Low-temperature ammoxidation catalyst and preparation method thereof
By adding molecular sieve material to the underlying precious metal coating, the thickness and diffusion resistance of the upper SCR coating are reduced, and NOx is reduced in the underlying precious metal coating, the problems of NH3 escape and by-product generation in existing catalysts are solved, and low-temperature NH3 is achieved Comprehensive effect of improving oxidative activity and reducing by-products.
Patent Information
- Application Number
- CN202411182823.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
AI Technical Summary
The existing NH3 selective catalytic reduction catalysts are difficult to contact the precious metal coating due to the diffusion resistance of the upper molecular sieve SCR coating, causing NH3 to escape and generate by-products NOx and N2O, which cannot meet the next generation and higher emission standards of National VI. .
By adding molecular sieve material to the underlying precious metal coating, the thickness and diffusion resistance of the upper SCR coating are reduced, and the generated NOx is reduced in the underlying precious metal coating, thereby reducing the formation of NOx and N2O.
It improves the oxidation activity of low-temperature NH3, reduces the generation of by-products NOx and N2O, meets the next generation and higher emission standards of National VI, and improves the performance of diesel vehicle exhaust treatment technology.
Smart Images

Figure CN118904384A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a low-temperature ammonia oxidation catalyst and a preparation method thereof. Background Art
[0002] Ammonia selective catalytic reduction (NH3-SCR) is a NO x Emission reduction technology that can be used to achieve strict NO x Emission targets. With NO x The emission limits are getting lower and lower, requiring the NH3-SCR catalyst to have a higher ammonia storage capacity or add more urea to achieve higher NO x Conversion rate. In addition, with the removal of engine EGR and the tightening of fuel consumption regulations, the exhaust temperature is lower, and the NH3 leakage temperature is lower than 250°C, and NH3 leakage brings many problems. NH3 is a toxic gas with a pungent odor. NH3 is also a promoter of haze and can promote the formation of secondary particulate matter. The National VI limit for NH3 emissions in heavy-duty vehicle exhaust is 10ppm. Ammonia slip catalyst (ASC) is a simple and efficient method to remove NH3 from diesel vehicle exhaust, but the generation of byproducts NO and N2O is a problem. NO x It is a toxic gas, and NO x The generation of N2O will reduce the catalytic efficiency of the SCR catalyst, and the greenhouse effect of N2O is more than 300 times that of CO2. Therefore, for ASC catalysts, in addition to considering the conversion rate of NH3 below 250°C, the product selectivity of NH3 oxidation must also be considered.
[0003] The commercially used ASC coating structure is a double-layer coating, including a bottom precious metal coating and an upper SCR coating. A portion of NH3 diffuses through the upper molecular sieve coating to the lower precious metal coating to be oxidized, producing a mixture of required N2 and unwanted N2O, NO and NO2, and then NO x The product diffuses to the upper layer and reacts with the reverse-diffused ammonia or stored ammonia in the molecular sieve coating to produce N2 by NH3-SCR reaction. Although the current commercial catalysts can greatly improve the N2 selectivity of the catalyst, there are still some problems. The general application conditions of ASC catalysts are high space velocity. Due to the diffusion resistance of the upper molecular sieve SCR coating, some pollutants NH3 are difficult to contact the precious metal coating, causing NH3 to escape. For this reason, the development of low-temperature NH3 oxidation performance is excellent and the by-product NO x The ASC with low N2O generation can meet the next generation of National VI and higher emission standards, which is of great significance for promoting the development of diesel vehicle exhaust after-treatment technology in my country. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a low-temperature ammonia oxidation catalyst, which places part of the molecular sieve on the bottom precious metal coating, reduces the coating thickness of the upper SCR coating, reduces the diffusion resistance, improves the low-temperature ammonia oxidation, and the molecular sieve on the bottom can reduce the byproduct NO x and N2O effects, thereby achieving the combined effect of enhancing low-temperature NH3 oxidation and reducing by-products.
[0005] The purpose of the present invention is mainly achieved through the following technical solutions:
[0006] In the first aspect, the present application proposes a low-temperature ammonia-oxygen catalyst, comprising a bottom precious metal coating and an upper SCR coating, wherein the bottom precious metal coating comprises a carrier material and a precious metal loaded on the carrier material, the carrier material comprises an acidic carrier and a molecular sieve, the upper SCR coating comprises a molecular sieve and an active component loaded on the molecular sieve, the loading amount of the bottom precious metal coating is 40-80 g / L, and the loading amount of the upper SCR coating is 70-130 g / L.
[0007] The technical problem to be solved by the present invention is that the existing commercial catalysts have difficulty in contacting the precious metal coating with some pollutants NH3 due to the diffusion resistance of the upper molecular sieve SCR coating, resulting in NH3 escaping. In this application, in order to reduce the diffusion resistance of the upper SCR coating, reduce the molecular sieve content in the upper SCR coating, thereby reducing the loading amount of the upper SCR coating, reducing the thickness of the upper SCR coating, and increasing the low-temperature NH3 oxidation activity, at the same time, in this application, molecular sieve materials are added to the bottom precious metal coating. When NH3 diffuses to the bottom precious metal coating and is oxidized, the byproduct NO x Can be reduced in the molecular sieve in the underlying noble metal coating, thereby reducing NO x The content of NO diffuses upward to the upper SCR coating, while x It is an intermediate in the production of N2O, reducing NO x It can reduce the generation of N2O, thereby reducing the by-product NO x In this application, by changing the distribution of molecular sieve materials and placing part of the molecular sieve in the bottom precious metal coating, the coating thickness of the upper SCR coating is reduced, the diffusion resistance is reduced, and the low-temperature ammonia oxidation is improved. At the same time, the molecular sieve at the bottom plays a role in reducing the byproduct NO x and N2O effects, thereby achieving the combined effect of enhancing low-temperature ammonia oxidation and reducing by-products.
[0008] Furthermore, the mass ratio of the acidic carrier to the molecular sieve is 1:1-5:1.
[0009] Furthermore, the acidic carrier includes any one of TiO2, Al2O3, TiO2-Al2O3, SiO2-Al2O3 and TiO2-SiO2-Al2O3.
[0010] Further, the molecular sieve in the bottom noble metal coating is any one of Beta, ZSM-5, CHA, AEI, FAU, LTA, and AFX. Preferably, the molecular sieve in the bottom noble metal coating is one of CHA or AEI.
[0011] Furthermore, the noble metal in the bottom noble metal coating is at least one of Pt and Pd.
[0012] Further, the molecular sieve in the upper SCR coating is any one of Beta, ZSM-5, CHA, AEI, FAU, LTA, AFX or a combination of at least two. Preferably, the molecular sieve in the upper SCR coating is one of CHA and AEI or a combination of two. Optionally, the molecular sieve in the bottom precious metal coating and the molecular sieve in the upper SCR coating can be the same material or different materials.
[0013] Furthermore, the active component is at least one of Cu ions and Fe ions, and the Cu ions and / or Fe ions account for 2.5wt%-5.5wt% of the mass of the molecular sieve.
[0014] Furthermore, the molar ratio of the molecular sieve silicon oxide to aluminum oxide is 5 to 25:1.
[0015] In a second aspect, the present application also proposes a method for preparing a low-temperature ammonia oxidation catalyst, which is used to prepare the low-temperature ammonia oxidation catalyst as described above, comprising the following steps:
[0016] Step 1: Prepare the bottom precious metal coating slurry by the over-impregnation method: mix the precious metal solution, the acidic carrier, the molecular sieve and the deionized water, stir them evenly and then add the adhesive, and after ball milling evenly, obtain the bottom precious metal coating slurry;
[0017] Step 2: Prepare the upper SCR coating slurry by ion exchange method: exchange the active component precursor onto the molecular sieve, filter, wash and dry at 80-120°C, and after drying, calcine at 500-600°C in air atmosphere for 1-3h to obtain the molecular sieve SCR coating; mix the molecular sieve SCR coating, adhesive and deionized water, and obtain the upper SCR coating slurry after ball milling;
[0018] Step 3: The bottom noble metal coating slurry and the upper SCR coating slurry are coated on the cordierite monolithic carrier respectively, and the ASC catalyst is obtained after drying and calcining.
[0019] In summary, the present invention has the following beneficial effects compared with the prior art: the present invention reduces the thickness of the upper SCR coating by adjusting the thickness of the upper SCR coating, thereby reducing the diffusion resistance, increasing the low-temperature ammonia oxidation activity, and better reflecting the true activity of the underlying precious metal coating; the present invention adds molecular sieve materials to the underlying precious metal coating, so that the underlying precious metal coating can not only have the ammonia oxidation function, but also reduce the byproduct NO x and N2O production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:
[0021] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0022] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0023] A low-temperature ammonia-oxygen catalyst comprises a bottom noble metal coating and an upper SCR coating, wherein the bottom noble metal coating comprises a carrier material and a noble metal loaded on the carrier material, the carrier material comprises an acidic carrier and a molecular sieve, the upper SCR coating comprises a molecular sieve and an active component loaded on the molecular sieve, the loading amount of the bottom noble metal coating is 40-80 g / L, and the loading amount of the upper SCR coating is 70-130 g / L.
[0024] The technical problem to be solved by this application is that the existing commercial catalysts have some pollutants NH3 that are difficult to contact the precious metal coating due to the diffusion resistance of the upper molecular sieve SCR coating, resulting in NH3 escape. In the embodiment of this application, in order to reduce the diffusion resistance of the upper SCR coating, reduce the molecular sieve content in the upper SCR coating, thereby reducing the loading amount of the upper SCR coating, reduce the thickness of the upper SCR coating, and increase the low-temperature NH3 oxidation activity. At the same time, in the embodiment of this application, molecular sieve materials are added to the bottom precious metal coating. When NH3 diffuses to the bottom precious metal coating and is oxidized, the byproduct NO x Can be reduced in the molecular sieve in the underlying noble metal coating, thereby reducing NO x The content of NO diffuses upward to the upper SCR coating, while x It is an intermediate in the production of N2O, reducing NO x It can reduce the generation of N2O, thereby reducing the by-product NOx In the embodiment of the present application, by changing the distribution of the molecular sieve material, part of the molecular sieve is placed in the bottom precious metal coating, the coating thickness of the upper SCR coating is reduced, the diffusion resistance is reduced, and the low-temperature ammonia oxidation is improved. At the same time, the molecular sieve at the bottom plays a role in reducing the byproduct NO x It should be noted that in the embodiments of the present application, the acidic carrier has a low ammonia storage capacity, which is mainly used to disperse the precious metals and increase the service life of the catalyst; the molecular sieve in the bottom precious metal coating has a high ammonia storage capacity, which, in addition to dispersing the precious metals, can also reduce NO x The amount of generation.
[0025] Furthermore, the mass ratio of the acidic carrier to the molecular sieve is 1:1-5:1.
[0026] Furthermore, the acidic carrier includes any one of TiO2, Al2O3, TiO2-Al2O3, SiO2-Al2O3 and TiO2-SiO2-Al2O3.
[0027] Further, the molecular sieve in the bottom noble metal coating is any one of Beta, ZSM-5, CHA, AEI, FAU, LTA, and AFX. Preferably, the molecular sieve in the bottom noble metal coating is one of CHA or AEI.
[0028] Furthermore, the noble metal in the bottom noble metal coating is at least one of Pt and Pd.
[0029] Further, the molecular sieve in the upper SCR coating is any one of Beta, ZSM-5, CHA, AEI, FAU, LTA, AFX or a combination of at least two. Preferably, the molecular sieve in the upper SCR coating is one of CHA and AEI or a combination of two. Optionally, the molecular sieve in the bottom precious metal coating and the molecular sieve in the upper SCR coating can be the same material or different materials.
[0030] Furthermore, the active component is at least one of Cu ions and Fe ions, and the Cu ions and / or Fe ions account for 2.5wt%-5.5wt% of the mass of the molecular sieve.
[0031] Furthermore, the molar ratio of the molecular sieve silicon oxide to aluminum oxide is 5 to 25:1.
[0032] Based on this, the present application also proposes a method for preparing a low-temperature ammonia oxidation catalyst, which is used to prepare the low-temperature ammonia oxidation catalyst as described above. Figure 1 As shown, the following steps are included:
[0033] Step 1: Prepare the bottom precious metal coating slurry by the over-impregnation method: mix the precious metal solution, the acidic carrier, the molecular sieve and the deionized water, stir them evenly and then add the adhesive, and after ball milling evenly, obtain the bottom precious metal coating slurry;
[0034] Step 2: Prepare the upper SCR coating slurry by ion exchange method: exchange the active component precursor onto the molecular sieve, filter, wash and dry at 80-120°C, and after drying, calcine at 500-600°C in air atmosphere for 1-3h to obtain the molecular sieve SCR coating; mix the molecular sieve SCR coating, adhesive and deionized water, and obtain the upper SCR coating slurry after ball milling;
[0035] Step 3: The bottom noble metal coating slurry and the upper SCR coating slurry are coated on the cordierite monolithic carrier respectively, and the ASC catalyst is obtained after drying and calcining.
[0036] It should be noted that when preparing the bottom precious metal coating slurry, except that the mass ratio of the acidic carrier and the molecular sieve is limited to 1:1-5:1, the content of the precious metal solution and deionized water is appropriately set according to the loading amount, and there is no specific ratio limit, so as to facilitate coating.
[0037] Embodiment 1:
[0038] Preparation of bottom precious metal coating slurry: Through the over-impregnation method, the precious metal solution (3g / ft 3 Pt), TiO2-Al2O3, SSZ-13 (Si / Al=8) and deionized water are fully mixed, and after being stirred evenly, a binder is added, and after ball milling evenly, a bottom precious metal coating slurry is obtained; wherein the mass ratio of TiO2-Al2O3 and SSZ-13 is TiO2-Al2O3:SSZ-13=1:1;
[0039] Preparation of upper SCR coating slurry: copper nitrate solution (containing 3.0wt% Cu) is loaded onto AEI (Si / Al=15) material by ion exchange method, filtered, washed and dried at 100°C, and then calcined at 500°C for 3h in air atmosphere to obtain molecular sieve SCR coating; molecular sieve SCR coating, adhesive and deionized water are mixed, and ball milled to obtain upper SCR coating slurry;
[0040] The bottom precious metal coating slurry is coated on a ceramic carrier with a size of "1in*1in" and a pore density of 400 mesh. The precious metal content is 3g / ft 3The loading amount is 45 g / L. After drying at 80°C, the upper SCR coating slurry is coated on the ceramic carrier containing the precious metal layer with a loading amount of 70 g / L. After drying at 80°C, it is calcined at 500°C in a muffle furnace for 2 hours to obtain an ASC catalyst, and the ASC catalyst is recorded as S1.
[0041] Embodiment 2:
[0042] This example is modified on the basis of Example 1. When preparing the bottom precious metal coating slurry, the mass ratio of TiO2-Al2O3 and SSZ-13 is changed to TiO2-Al2O3:SSZ-13=3:1, and the obtained ASC catalyst is recorded as S2.
[0043] Embodiment 3:
[0044] This example is modified on the basis of Example 1. When preparing the bottom precious metal coating slurry, the mass ratio of TiO2-Al2O3 and SSZ-13 is changed to TiO2-Al2O3:SSZ-13=5:1. The obtained ASC catalyst is recorded as S3.
[0045] Embodiment 4:
[0046] This example is modified on the basis of Example 1. When preparing the ASC catalyst, the loading amount of the upper SCR coating is modified to 100 g / L. The obtained ASC catalyst is recorded as S4.
[0047] Embodiment 5:
[0048] This example is modified on the basis of Example 1. When preparing the ASC catalyst, the loading amount of the upper SCR coating is modified to 130 g / L. The obtained ASC catalyst is recorded as S5.
[0049] Embodiment 6:
[0050] This example is modified on the basis of Example 1. When preparing the ASC catalyst, the loading amount of the bottom precious metal coating is modified to 80 g / L. The obtained ASC catalyst is recorded as S6.
[0051] Embodiment 7:
[0052] This example is modified on the basis of Example 1. When preparing the bottom precious metal coating slurry, the mass ratio of TiO2-Al2O3 and SSZ-13 is changed to TiO2-Al2O3:SSZ-13=5:1. When preparing the ASC catalyst, the loading amount of the upper SCR coating is changed to 130g / L. The obtained ASC catalyst is recorded as S7.
[0053] Comparative Example 1:
[0054] Preparation of bottom precious metal coating slurry: Through the over-impregnation method, the precious metal solution (3g / ft 3 Pt), TiO2-Al2O3 carrier material and deionized water are fully mixed, and after being stirred evenly, a binder is added, and after ball milling evenly, a bottom noble metal coating slurry is obtained;
[0055] Preparation of upper SCR coating slurry: the same as the preparation method of the upper SCR coating slurry in Example 1;
[0056] The bottom precious metal coating slurry is coated on a ceramic carrier with a size of "1in*1in" and a pore density of 400 mesh. The precious metal content is 3g / ft 3 The loading amount is 45 g / L. After drying at 80°C, the upper SCR coating slurry is coated on the ceramic carrier containing the precious metal layer with a loading amount of 70 g / L. After drying at 80°C, it is calcined at 500°C in a muffle furnace for 2 hours to obtain an ASC catalyst, and the ASC catalyst is recorded as B1.
[0057] Comparative Example 2:
[0058] This comparative example was modified on the basis of Example 1. When preparing the ASC catalyst, the loading amount of the upper SCR coating was modified to 150 g / L. The obtained ASC catalyst was recorded as B2.
[0059] Comparative Example 3:
[0060] This comparative example was modified on the basis of Example 1. When preparing the ASC catalyst, the loading amount of the upper SCR coating was modified to 65 g / L. The obtained ASC catalyst was recorded as B3.
[0061] Comparative Example 4:
[0062] This comparative example is modified on the basis of Example 7. When preparing the ASC catalyst, when preparing the underlying precious metal coating slurry, the mass ratio of TiO2-Al2O3 and SSZ-13 is modified to TiO2-Al2O3:H-SSZ-13=7:1, and the obtained ASC catalyst is recorded as B4.
[0063] The ASC catalysts prepared in Examples 1 to 7 and Comparative Examples 1 to 4 were tested for NH3 conversion efficiency in a fixed bed reactor:
[0064] The simulated gas composition during the test was: [NH3] = 500ppm, [O2] = 10%, [H2O] = 7%, N2 as the balance gas, and the air velocity was 150000h -1 , the reaction temperature is 200° C., 250° C., and 500° C. The ammonia oxidation results of Examples 1-7 and Comparative Examples 1-4 are shown in Table 1 below:
[0065] Table 1:
[0066]
[0067]
[0068] As can be seen from Table 1, adding part of the molecular sieve material in the upper SCR coating to the bottom precious metal coating can reduce the thickness of the upper SCR coating while reducing the diffusion resistance and improving the NH3 oxidation activity. At the same time, the molecular sieve at the bottom can reduce the byproduct NO x When the mass ratio of the acidic carrier material to the molecular sieve material is 5:1 and the loading amount of the upper SCR coating is 70g / L, the comprehensive effect of NH3 oxidation and selectivity is optimal. If the amount of molecular sieve in the bottom precious metal coating is further increased, the oxidation activity of NH3 will decrease, and the loading amount of the upper SCR coating will be reduced, then the byproduct NO x Increased selectivity.
[0069] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A low-temperature ammonia-oxygen catalyst, comprising a bottom noble metal coating and an upper SCR coating, characterized in that: The bottom layer precious metal coating comprises a carrier material and a precious metal loaded on the carrier material, the carrier material comprises an acidic carrier and a molecular sieve, the upper layer SCR coating comprises a molecular sieve and an active component loaded on the molecular sieve, the loading amount of the bottom layer precious metal coating is 40-80 g / L, and the loading amount of the upper layer SCR coating is 70-130 g / L.
2. A low-temperature ammonia oxidation catalyst according to claim 1, characterized in that: The mass ratio of the acidic carrier to the molecular sieve is 1:1-5:
1.
3. A low-temperature ammonia oxidation catalyst according to claim 1, characterized in that: The acidic carrier includes any one of TiO2, Al2O3, TiO2-Al2O3, SiO2-Al2O3 and TiO2-SiO2-Al2O3.
4. A low-temperature ammonia oxidation catalyst according to claim 1, characterized in that: The molecular sieve in the bottom precious metal coating is any one of Beta, ZSM-5, CHA, AEI, FAU, LTA, and AFX.
5. A low-temperature ammonia oxidation catalyst according to claim 1, characterized in that: The noble metal in the bottom noble metal coating is at least one of Pt and Pd.
6. A low-temperature ammonia oxidation catalyst according to claim 1, characterized in that: The molecular sieve in the upper SCR coating is any one of Beta, ZSM-5, CHA, AEI, FAU, LTA, and AFX, or a combination of at least two thereof.
7. A low-temperature ammonia oxidation catalyst according to claim 1, characterized in that: The active component is at least one of Cu ions and Fe ions, and the Cu ions and / or Fe ions account for 2.05wt%-5.5wt% of the mass of the molecular sieve.
8. A low-temperature ammonia oxidation catalyst according to claim 1, characterized in that: The molar ratio of the molecular sieve silicon oxide to aluminum oxide is 5 to 25:
1.
9. A method for preparing a low-temperature ammonia oxidation catalyst, characterized in that: The method for preparing the low-temperature ammonia oxidation catalyst according to any one of claims 1 to 8 comprises the following steps: Step 1: preparing the bottom precious metal coating slurry: by using the over-impregnation method, the precious metal solution, the acidic carrier, the molecular sieve and the deionized water are mixed, and after stirring evenly, the adhesive is added, and after ball milling evenly, the bottom precious metal coating slurry is obtained; Step 2: Prepare the upper SCR coating slurry: exchange the active component precursor onto the molecular sieve by ion exchange method, filter, wash and dry at 80-120°C, and after drying, calcine at 500-600°C in air atmosphere for 1-3h to obtain the molecular sieve SCR coating; mix the molecular sieve SCR coating, adhesive and deionized water, and obtain the upper SCR coating slurry after ball milling; Step 3: The bottom noble metal coating slurry and the upper SCR coating slurry are coated on the cordierite monolithic carrier respectively, and the ASC catalyst is obtained after drying and calcining.
Citation Information
Cited By
Supported low-temperature ammoxidation reaction catalyst, preparation method and application
CN119864431A
Supported low-temperature ammonia oxidation reaction catalyst, preparation method and application
CN119864431B