Preparation method and application of nitrogen-containing super-crosslinked polymer loaded Pd nanoparticle catalyst
By using a nitrogen-containing supercrosslinked polymer-supported Pd nanoparticle catalyst in the palladium nanoparticle catalyst, the problems of low specific surface area of the palladium nanoparticle supported catalyst and easy deactivation of the catalyst are solved, and the performance of the catalyst and the efficiency of formic acid decomposition reaction are improved.
Patent Information
- Application Number
- CN202410970913.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The specific surface area of existing palladium nanoparticle supported catalysts is low and prone to inactivation due to agglomeration. The pore size structure optimization of aromatic amine-based supercrosslinked polymers has limited improvement in the performance of the catalyst, limiting its application in formic acid decomposition catalysis.
The preparation method of the nitrogen-containing supercrosslinked polymer supported Pd nanoparticle catalyst is adopted. By adjusting the reaction conditions and selecting suitable crosslinking agents and reducing agents, the specific surface area and activity of the catalyst are improved, and the iron species in the carrier are retained to enhance catalysis. performance.
The specific surface area and catalytic activity of the catalyst are significantly improved, the synthesis process is simplified, and the performance of the catalyst is further improved by retaining iron species, achieving efficient catalysis of formic acid decomposition.
Smart Images

Figure CN118904391A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal catalysis, and in particular relates to a preparation method and application of a nitrogen-containing super-crosslinked polymer-loaded Pd nanoparticle catalyst. Background Art
[0002] Among the many hydrogen storage materials, formic acid has received a lot of attention in recent years due to its advantages such as easy availability, easy storage and transportation, high hydrogen volume density, and non-toxicity. Palladium-based supported heterogeneous catalysts are currently the most common heterogeneous catalysts for the decomposition of formic acid. However, the catalyst still faces problems such as low activity and further deactivation due to agglomeration. The introduction of catalyst carriers can effectively improve this problem. However, compared with practical applications, the porous carriers currently used for palladium nanoparticle loading still need to be improved. For example, the catalyst used for palladium nanoparticle loading should have a higher specific surface area to achieve efficient loading of palladium nanoparticles, and there should also be a large number of dispersed heteroatoms on the carrier to fix the palladium nanoparticles loaded thereon.
[0003] Braided hyper-crosslinked polymers are a traditional porous organic polymer material that has attracted a lot of attention in the field of gas adsorption due to their excellent pore structure. However, there are still many shortcomings in heteroatom-containing porous materials used as catalyst carriers. Specifically, when aromatic amines (such as aniline, phenylenediamine, etc.) are used to synthesize hyper-crosslinked polymers, the product will significantly reduce its specific surface area due to the influence of reaction activity and intermolecular interactions. In order to solve this problem, many attempts have been made. Although the aromatic amine-benzene co-crosslinking method can effectively increase the specific surface area of the carrier, it will reduce the heteroatom content of the carrier. The modification strategy for reaction conditions currently has limited effect on the improvement of catalyst performance. Therefore, there is still great potential for the synthesis and optimization of the pore structure of aromatic amine-based hyper-crosslinked polymers, which also limits its space for palladium nanoparticle loading.
[0004] Therefore, the prior art urgently needs a new technical solution to solve the above problems. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a preparation method and application of a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst, prepare a palladium-based multiphase catalyst with a higher specific surface area, and improve the catalytic performance of a formic acid catalyst.
[0006] A method for preparing a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst comprises the following steps:
[0007] Step 1, adding a nitrogen-containing aromatic monomer and a cross-linking agent into an organic solvent, adding a Lewis acid catalyst after fully dissolving them to carry out a full cross-linking reaction, washing and drying after the reaction is completed to obtain a nitrogen-containing hyper-cross-linked polymer;
[0008] Step 2, stirring and mixing the nitrogen-containing hyper-crosslinked polymer and the chloropalladic acid solution, and then performing liquid phase separation to obtain the nitrogen-containing hyper-crosslinked polymer adsorbing palladium ions;
[0009] Step 3: The nitrogen-containing hyper-crosslinked polymer adsorbing palladium ions is fully reduced with a reducing agent, and the hyper-crosslinked polymer loaded with Pd species is obtained by liquid phase separation.
[0010] The nitrogen-containing aromatic monomer is anhydrous m-phenylenediamine; the cross-linking agent is anhydrous dimethoxymethane; the organic solvent is anhydrous ethylene dichloride; and the Lewis acid catalyst is anhydrous ferric chloride.
[0011] The molar ratio of the nitrogen aromatic monomer to the crosslinking agent is 1:1-1.5; the volume of the organic solvent per mole of the nitrogen aromatic monomer is 600-700 mL; and the molar ratio of the crosslinking agent to the Lewis acid catalyst is 1:0.2-0.4.
[0012] The washing adopts one or a mixed solvent of water and ethanol.
[0013] The concentration of the chloropalladic acid solution is 0.01 mol / L, and the volume of the chloropalladic acid solution per gram of nitrogen-containing hyper-crosslinked polymer is 30 ml. After adding chloropalladic acid, the solution is diluted to 200 ml.
[0014] The nitrogen-containing hyper-crosslinked polymer and the chloropalladic acid solution are stirred at a speed of 6000-8000 r / min.
[0015] The reducing agent is sodium borohydride. The mass of sodium borohydride required for each gram of nitrogen-containing hyper-crosslinked polymer is 400 mg. After adding sodium borohydride, the solution is diluted to 200 ml.
[0016] The invention discloses an application of a Pd nanoparticle catalyst supported by a nitrogen-containing hyper-crosslinked polymer, which is used to catalyze the decomposition of formic acid.
[0017] Through the above-mentioned design scheme, the present invention can bring the following beneficial effects: a preparation method and application of a nitrogen-containing hyper-cross-linked polymer-loaded Pd nanoparticle catalyst, which effectively improves the specific surface area of the prepared hyper-cross-linked polymer by adjusting different reaction conditions, and makes the conditions of its synthesis reaction milder; subsequently, this work successfully improved the catalytic activity of the prepared catalyst by increasing the specific surface area of the hyper-cross-linked polymer carrier, and the performance was significantly improved compared with previous synthesis methods.
[0018] Furthermore, the present invention further improves the activity of the catalyst by retaining some iron species remaining in the catalyst carrier. In addition, the proper retention of iron species is also conducive to the simplification of the catalyst synthesis process. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The present invention is further described below with reference to the accompanying drawings and specific embodiments:
[0020] Figure 1 This is a transmission electron microscope image of a palladium-based heterogeneous catalyst supported by a nitrogen-containing hyper-crosslinked polymer prepared in an embodiment of the present invention and a particle size distribution diagram of palladium nanoparticles supported thereon.
[0021] Figure 2 This is a transmission electron microscope image of the palladium-based heterogeneous catalyst supported by the nitrogen-containing hyper-crosslinked polymer prepared in Comparative Example 2 of the present invention and a particle size distribution diagram of the palladium nanoparticles supported by it.
[0022] Figure 3 It is a nitrogen adsorption-desorption curve diagram of the nitrogen-containing hyper-crosslinked polymer prepared in the embodiment of the present invention, comparative example 1 and comparative example 2.
[0023] Figure 4 It is a nitrogen adsorption-desorption curve diagram of the nitrogen-containing hyper-crosslinked polymer prepared in Example 3 and Comparative Example 4 of the present invention.
[0024] Figure 5 This is a graph showing the change over time of the gas generated by the decomposition of formic acid catalyzed by the palladium-based heterogeneous catalyst supported by the nitrogen-containing hyper-crosslinked polymer prepared in Examples of the present invention, Comparative Example 1 and Comparative Example 2.
[0025] Figure 6 This is a graph showing the change over time of the gas generated by the decomposition of formic acid catalyzed by the palladium-based heterogeneous catalyst supported by the nitrogen-containing hyper-cross-linked polymer prepared in Examples of the present invention, Comparative Examples 3 and 4.
[0026] Figure 7 This is a graph showing the change over time of the gas generated by the decomposition of formic acid catalyzed by the palladium-based heterogeneous catalyst supported by the nitrogen-containing hyper-crosslinked polymer prepared in Example 1 of the present invention and Comparative Example 5. DETAILED DESCRIPTION
[0027] The following combination Figure 1-Figure 7 The preparation method and application of the nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst of the present invention are further described.
[0028] Embodiment:
[0029] A method for preparing a palladium-based catalyst supported by a nitrogen-containing hyper-crosslinked polymer with a high specific surface area mainly comprises the following steps:
[0030] (1) In a 100-mL round-bottom flask, 12.5 mL of anhydrous dichloroethane, 2.16 g of m-phenylenediamine (20 mmol), and 2.21 mL of dimethoxymethane (25 mmol) were added in sequence and stirred evenly to dissolve and disperse the mixture.
[0031] (2) Add 1.01 g of anhydrous ferric chloride, then stir vigorously, disperse evenly, and react at 30° C. for 24 hours.
[0032] (3) The resulting mixed phase was washed several times by centrifugation with ultrapure water and ethanol, respectively, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer. The physical adsorption method showed that its specific surface area was 23.1 m 2 ·g -1 .
[0033] (4) 100 mg of nitrogen-containing hyper-crosslinked polymer was weighed and dispersed in 20 mL of water, 3 mL of chloropalladic acid solution (containing 0.03 mmol of chloropalladic acid) was added, and then stirred at room temperature for 8 hours. After loading the palladium species, the material was centrifuged and washed with anhydrous ethanol, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium ions.
[0034] Ultrasonic dispersion of the nitrogen-containing hyper-crosslinked polymer loaded with palladium ions in an appropriate amount of water and rapid addition of 2 mL of freshly prepared sodium borohydride solution (containing 40 mg of sodium borohydride), followed by addition of water to 20 mL and vigorous stirring at room temperature for 6 hours. After the reduction reaction is completed, centrifuge and wash with a small amount of ethanol. Finally, dry overnight in a vacuum oven at 333 K to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium nanoparticles. The results of inductively coupled plasma spectroscopy show that the mass proportion of palladium loaded on the catalyst is 3.09%, and the results of transmission electron microscopy show that the average particle size of the palladium nanoparticles loaded on the catalyst is 1.21 nanometers, as shown in FIG. Figure 1 shown.
[0035] Comparative Example 1:
[0036] This comparative example provides a method for preparing a nitrogen-containing hyper-crosslinked polymer-supported palladium-based catalyst, which mainly comprises the following steps:
[0037] (1) In a 100-mL round-bottom flask, 12.5 mL of anhydrous dichloroethane, 2.16 g of m-phenylenediamine (20 mmol), and 2.21 mL of dimethoxymethane (25 mmol) were added in sequence and stirred evenly to dissolve and disperse the mixture.
[0038] (2) Add 2.02 g of anhydrous ferric chloride, then stir vigorously, disperse evenly, and react at 30° C. for 24 hours.
[0039] (3) The resulting mixed phase was washed several times by centrifugation with ultrapure water and ethanol, respectively, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer. The physical adsorption method showed that its specific surface area was 23.1 m 2 ·g -1 .
[0040] (4) 100 mg of nitrogen-containing hyper-crosslinked polymer was weighed and dispersed in 20 mL of water, 3 mL of chloropalladic acid solution (containing 0.03 mmol of chloropalladic acid) was added, and then stirred at room temperature for 8 hours. After loading the palladium species, the material was centrifuged and washed with anhydrous ethanol, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium ions.
[0041] The nitrogen-containing hyper-crosslinked polymer loaded with palladium ions was ultrasonically dispersed in an appropriate amount of water and 2 mL of freshly prepared sodium borohydride solution (containing 40 mg of sodium borohydride) was quickly added, followed by adding water to 20 mL and vigorously stirring at room temperature for 6 hours. After the reduction reaction was completed, the mixture was centrifuged and washed with a small amount of ethanol. Finally, it was dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium nanoparticles.
[0042] Comparative Example 2:
[0043] This comparative example provides a method for preparing a nitrogen-containing hyper-crosslinked polymer-supported palladium-based catalyst, which mainly comprises the following steps:
[0044] (1) In a 100-mL round-bottom flask, 12.5 mL of anhydrous dichloroethane, 2.16 g of m-phenylenediamine (20 mmol), and 2.21 mL of dimethoxymethane (25 mmol) were added in sequence and stirred evenly to dissolve and disperse the mixture.
[0045] (2) Add 4.05 g of anhydrous ferric chloride, then stir vigorously, disperse evenly, and react at 30° C. for 24 hours.
[0046] (3) The obtained mixed phase was washed several times by centrifugation with ultrapure water and ethanol respectively, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer. The physical adsorption method showed that its specific surface area was 23.1 m2·g-1.
[0047] (4) 100 mg of nitrogen-containing hyper-crosslinked polymer was weighed and dispersed in 20 mL of water, 3 mL of chloropalladic acid solution (containing 0.03 mmol of chloropalladic acid) was added, and then stirred at room temperature for 8 hours. After loading the palladium species, the material was centrifuged and washed with anhydrous ethanol, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium ions.
[0048] Ultrasonic dispersion of the nitrogen-containing hyper-crosslinked polymer loaded with palladium ions in an appropriate amount of water and rapid addition of 2 mL of freshly prepared sodium borohydride solution (containing 40 mg of sodium borohydride), followed by addition of water to 20 mL and vigorous stirring at room temperature for 6 hours. After the reduction reaction is completed, centrifuge and wash with a small amount of ethanol. Finally, dry overnight in a vacuum oven at 333 K to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium nanoparticles. The results of inductively coupled plasma spectroscopy show that the mass proportion of palladium loaded on the catalyst is 3.09%, and the results of transmission electron microscopy show that the average particle size of the palladium nanoparticles loaded on the catalyst is 1.51 nanometers, as shown in FIG. Figure 2 shown.
[0049] Comparative Example 3:
[0050] This comparative example provides a method for preparing a nitrogen-containing hyper-crosslinked polymer-supported palladium-based catalyst, which mainly comprises the following steps:
[0051] (1) In a 100-mL round-bottom flask, 12.5 mL of anhydrous dichloroethane, 2.16 g of m-phenylenediamine (20 mmol), and 2.21 mL of dimethoxymethane (25 mmol) were added in sequence and stirred evenly to dissolve and disperse the mixture.
[0052] (2) Add 1.01 g of anhydrous ferric chloride, then stir vigorously, disperse evenly, and react at 55° C. for 24 hours.
[0053] (3) The resulting mixed phase was washed several times by centrifugation with ultrapure water and ethanol, respectively, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer. The physical adsorption method showed that its specific surface area was 23.1 m 2 ·g -1 .
[0054] (4) 100 mg of nitrogen-containing hyper-crosslinked polymer was weighed and dispersed in 20 mL of water, 3 mL of chloropalladic acid solution (containing 0.03 mmol of chloropalladic acid) was added, and then stirred at room temperature for 8 hours. After loading the palladium species, the material was centrifuged and washed with anhydrous ethanol, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium ions.
[0055] The nitrogen-containing hyper-crosslinked polymer loaded with palladium ions was ultrasonically dispersed in an appropriate amount of water and 2 mL of freshly prepared sodium borohydride solution (containing 40 mg of sodium borohydride) was quickly added, followed by adding water to 20 mL and vigorously stirring at room temperature for 6 hours. After the reduction reaction was completed, the mixture was centrifuged and washed with a small amount of ethanol. Finally, it was dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium nanoparticles.
[0056] Comparative Example 4:
[0057] This comparative example provides a method for preparing a nitrogen-containing hyper-crosslinked polymer-supported palladium-based catalyst, which mainly comprises the following steps:
[0058] (1) In a 100-mL round-bottom flask, 12.5 mL of anhydrous dichloroethane, 2.16 g of m-phenylenediamine (20 mmol), and 2.21 mL of dimethoxymethane (25 mmol) were added in sequence and stirred evenly to dissolve and disperse the mixture.
[0059] (2) Add 1.01 g of anhydrous ferric chloride, then stir vigorously, disperse evenly, and react at 80° C. for 24 hours.
[0060] (3) The resulting mixed phase was washed several times by centrifugation with ultrapure water and ethanol, respectively, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer. The physical adsorption method showed that its specific surface area was 23.1 m 2 ·g -1 .
[0061] (4) 100 mg of nitrogen-containing hyper-crosslinked polymer was weighed and dispersed in 20 mL of water, 3 mL of chloropalladic acid solution (containing 0.03 mmol of chloropalladic acid) was added, and then stirred at room temperature for 8 hours. After loading the palladium species, the material was centrifuged and washed with anhydrous ethanol, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium ions.
[0062] The nitrogen-containing hyper-crosslinked polymer loaded with palladium ions was ultrasonically dispersed in an appropriate amount of water and 2 mL of freshly prepared sodium borohydride solution (containing 40 mg of sodium borohydride) was quickly added, followed by adding water to 20 mL and vigorously stirring at room temperature for 6 hours. After the reduction reaction was completed, the mixture was centrifuged and washed with a small amount of ethanol. Finally, it was dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium nanoparticles.
[0063] Comparative Example 5:
[0064] This comparative example provides a method for preparing a nitrogen-containing hyper-crosslinked polymer-supported palladium-based catalyst, which mainly comprises the following steps:
[0065] (1) In a 100-mL round-bottom flask, 12.5 mL of anhydrous dichloroethane, 2.16 g of m-phenylenediamine (20 mmol), and 2.21 mL of dimethoxymethane (25 mmol) were added in sequence and stirred evenly to dissolve and disperse the mixture.
[0066] (2) Add 1.01 g of anhydrous ferric chloride, then stir vigorously, disperse evenly, and react at 30° C. for 24 hours.
[0067] (3) The obtained mixed phase was washed several times by centrifugation with ultrapure water and ethanol, and then the obtained carrier was Soxhlet extracted with methanol for 48 hours. After the Soxhlet extraction, the hyper-crosslinked polymer product was dried in a vacuum oven at 333K overnight to obtain a nitrogen-containing hyper-crosslinked polymer. The physical adsorption method showed that its specific surface area was 23.1m 2 ·g -1 .
[0068] (4) 100 mg of nitrogen-containing hyper-crosslinked polymer was weighed and dispersed in 20 mL of water, 3 mL of chloropalladic acid solution (containing 0.03 mmol of chloropalladic acid) was added, and then stirred at room temperature for 8 hours. After loading the palladium species, the material was centrifuged and washed with anhydrous ethanol, and then dried in a vacuum oven at 333 K overnight to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium ions.
[0069] The nitrogen-containing hyper-crosslinked polymer loaded with palladium ions was ultrasonically dispersed in an appropriate amount of water and 2 mL of freshly prepared sodium borohydride solution (containing 40 mg of sodium borohydride) was quickly added, followed by adding water to 20 mL and vigorously stirring at room temperature for 6 hours. After the reduction reaction was completed, centrifuge and wash with a small amount of ethanol. Finally, dry overnight in a vacuum oven at 333K to obtain a nitrogen-containing hyper-crosslinked polymer loaded with palladium nanoparticles. The results of inductively coupled plasma spectroscopy showed that the mass proportion of palladium loaded by the catalyst was 3.09%, and the results of transmission electron microscopy showed that the average particle size of the palladium nanoparticles loaded by the catalyst was 1.51 nanometers.
[0070] Test example 1:
[0071] This test example uses N2 physical adsorption test to test the specific surface area of different palladium-based heterogeneous catalyst supports, and uses the Brunauer-Emmet-Teller (BET) method to determine the surface area of the catalyst. About 100 mg of sample was weighed for each test and vacuum dried at 50°C overnight to remove moisture before testing.
[0072] like Figure 3-Figure 7 As shown in the test results, the specific surface area of the hyper-crosslinked polymer synthesized in the embodiment is 23.1 m 2 ·g -1 , which is different from the embodiment, after increasing the amount of anhydrous ferric chloride catalyst, the specific surface areas of the hyper-crosslinked polymers synthesized in Comparative Example 1 and Comparative Example 2 were reduced to 2.4 m 2 ·g -1 and 1.6m 2 ·g -1 After increasing the synthesis temperature of the catalyst support, the specific surface area of the hyper-crosslinked polymers synthesized in Comparative Examples 3 and 4 was reduced to 16.1 m 2 ·g -1 and 15.8m 2 ·g-1 .
[0073] Test Example 2:
[0074] This test example tests the activity of different palladium-based heterogeneous catalysts in catalyzing the formic acid decomposition reaction.
[0075] (1) 50 mg of a palladium-based heterogeneous catalyst and 9.5 mL of ultrapure water were added to a round-bottom flask, and the reaction system was placed in an oil bath at 50°C and stirred continuously until the temperature of the reaction system reached 50°C.
[0076] (2) Rapidly inject 0.5 mL of 4 mol / L formic acid into the reaction system, collect the generated gas by water pressure method, and observe the volume of the liquid level in the gas cylinder that decreases over a certain period of time. Calculate the catalytic conversion rate using the reaction time-generated gas volume curve:
[0077]
[0078] Where P0 is the standard atmospheric pressure (101,325Pa), V is the amount of gas released when FA is converted to 20% (m 3 ), R represents the ideal gas constant (8.3145m 3 Pamol -1 K -1 ). T is the ambient temperature (298K), n Pd is the amount of Pd in the catalyst (mol), and t is the reaction time required to produce the corresponding gas (h).
[0079] The test results show that the multiphase catalyst of the embodiment can catalyze formic acid in the reaction system to produce 79.2 mL of gas within 8 minutes, with a conversion rate of 81% and a TOF value of up to 1486 h -1 Different from the embodiment, after increasing the dosage of the catalyst anhydrous ferric chloride, the TOF value of the heterogeneous catalyst for the decomposition of formic acid in Comparative Example 1 and Comparative Example 2 was reduced to 716.8 h -1 and 579.5h -1 After increasing the synthesis temperature of the catalyst support, the TOF value of the heterogeneous catalysts in Comparative Examples 3 and 4 for the decomposition of formic acid decreased to 1025.1h -1 and 517.3h -1 At the same time, after Soxhlet extraction, the TOF value of formic acid decomposition catalyzed by the heterogeneous catalyst of Comparative Example 5 was reduced to 1044h -1 .
[0080] The above conclusions show that the pore structure of the palladium nanoparticle carriers synthesized in different embodiments and comparative examples has a great influence on the performance of the prepared catalysts, and the increase in the specific surface area of the catalyst carrier is conducive to improving the catalytic performance of the prepared catalyst.
[0081] The above conclusions also show that some iron species remaining on the catalyst carrier are also beneficial to the improvement of catalytic performance.
[0082] The above description is only an implementation mode of the present invention. It should be pointed out that, for ordinary technicians in this field, improvements can be made without departing from the creative concept of the present invention, but these all belong to the protection scope of the present invention.
Claims
1. A method for preparing a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst, characterized in that: The following steps are included: Step 1, adding a nitrogen-containing aromatic monomer and a cross-linking agent into an organic solvent, adding a Lewis acid catalyst after fully dissolving them to carry out a full cross-linking reaction, washing and drying after the reaction is completed to obtain a nitrogen-containing hyper-cross-linked polymer; Step 2, stirring and mixing the nitrogen-containing hyper-crosslinked polymer and the chloropalladic acid solution, and then performing liquid phase separation to obtain the nitrogen-containing hyper-crosslinked polymer adsorbing palladium ions; Step 3: The nitrogen-containing hyper-crosslinked polymer adsorbing palladium ions is fully reduced with a reducing agent, and the hyper-crosslinked polymer loaded with Pd species is obtained by liquid phase separation.
2. The method for preparing a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst according to claim 1, characterized in that: The nitrogen-containing aromatic monomer is anhydrous m-phenylenediamine; the cross-linking agent is anhydrous dimethoxymethane; the organic solvent is anhydrous ethylene dichloride; and the Lewis acid catalyst is anhydrous ferric chloride.
3. The method for preparing a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst according to claim 1, characterized in that: The molar ratio of the nitrogen aromatic monomer to the crosslinking agent is 1:1-1.5; the volume of the organic solvent per mole of the nitrogen aromatic monomer is 600-700 mL; and the molar ratio of the crosslinking agent to the Lewis acid catalyst is 1:0.2-0.
4.
4. The method for preparing a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst according to claim 1, characterized in that: The washing adopts one or a mixed solvent of water and ethanol.
5. The method for preparing a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst according to claim 1, characterized in that: The concentration of the chloropalladic acid solution is 0.01 mol / L, and the volume of the chloropalladic acid solution per gram of nitrogen-containing hyper-crosslinked polymer is 30 ml. After adding chloropalladic acid, the solution is diluted to 200 ml.
6. The method for preparing a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst according to claim 1, characterized in that: The nitrogen-containing hyper-crosslinked polymer and the chloropalladic acid solution are stirred at a speed of 6000-8000 r / min.
7. The method for preparing a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst according to claim 1, characterized in that: The reducing agent is sodium borohydride. The mass of sodium borohydride required for each gram of nitrogen-containing hyper-crosslinked polymer is 400 mg. After adding sodium borohydride, the solution is diluted to 200 ml.
8. An application of a nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst, characterized in that: A nitrogen-containing hyper-crosslinked polymer-supported Pd nanoparticle catalyst prepared according to claim 1 is used to catalyze the decomposition of formic acid.
Citation Information
Patent Citations
Amino type porous polymer as well preparation method and application thereof
CN109517211A
Preparation method of palladium / amino-rich porous polymer catalyst for catalyzing self-decomposition of formic acid to prepare hydrogen
CN111346677A
Preparation method and application of aniline group modified MXene supported metal catalyst
CN114950544A
Method for preparing single-site catalyst based on triazine covalent framework material (CTFs)
CN116496496A
Catalyst for dehydrogenation reaction of formate and hydrogenation reaction of bicarbonate and preparation method thereof
US20180085738A1