Preparation method of catalyst for treating acrylonitrile sewage through microwave synergistic Fenton

By forming Cu2O(C4H8O)2(C14H12O)2 organic compound layer on the surface of the foam copper matrix and anchoring the ferrous composite hydride, combined with microwave treatment, the problems of low degradation rate and limited pH range in acrylonitrile wastewater treatment are solved. , achieving efficient COD removal and wide pH adaptability.

CN118904397APending Publication Date: 2024-11-08NORTH CHINA UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411057140.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has low degradation rate when treating acrylonitrile wastewater, and the chemical oxygen demand (COD) removal rate is not ideal, and the application range is limited by the acidic pH range, making it difficult to meet the treatment requirements of wide pH conditions.

Method used

Using microwave synergistic Fenton treatment method, CuO(C4H8O)4 organic compound layer is formed on the surface of the foam copper matrix, and converted into Cu2O(C4H8O)2(C14H12O)2 through copper ion conversion and diphenylacetaldehyde substitution. The organic compound layer is then anchored to the ferrous composite hydride [Fe(C14H14O2N)6](BH4)2 to form a catalyst to improve the oxidative degradation effect of acrylonitrile.

Benefits of technology

It achieves a high acrylonitrile/chemical oxygen demand (COD) removal rate, adapts to wide pH treatment conditions, and demonstrates excellent reusable performance, significantly improving the effect of acrylonitrile wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904397A_ABST
    Figure CN118904397A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a catalyst for treating acrylonitrile sewage through microwave synergistic Fenton. The preparation method comprises the following steps: forming a CuO (C4H8O) 4 organic compound layer on the surface of a foamy copper matrix; the CuO (C4H8O) 4 organic compound layer on the surface of the foamy copper is converted into a Cu2O (C4H8O) 2 (C14H12O) 2 organic compound layer through copper ion conversion and biphenyl acetaldehyde group substitution; and a ferrous composite hydride [Fe (C14H14O2N) 6] (BH4) 2 is anchored on the surface of the Cu2O (C4H8O) 2 (C14H12O) 2 organic compound layer. The catalyst prepared by the method provided by the invention has high acrylonitrile / chemical oxygen demand (COD) removal rate, wide pH applicability and excellent reusability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sewage treatment, in particular to a method for preparing a catalyst for treating acrylonitrile sewage by microwave-assisted Fenton treatment. Background Art

[0002] Acrylonitrile wastewater mainly comes from the production process of acrylonitrile, including acrylonitrile production process, acrylic fiber production process and ABS plastic production wastewater. Acrylonitrile wastewater is highly toxic and can cause serious damage to human skin, respiratory system, nervous system, and digestive system. It may also cause cancer and teratogenic risks. Acrylonitrile wastewater has a high chemical oxygen demand (COD) and is difficult to degrade. It is not only harmful to human health, but also causes serious pollution to the ecological environment.

[0003] Fenton treatment is a chain reaction between ferrous ions and hydrogen peroxide to produce hydroxyl radicals with oxidation ability, thereby degrading organic matter contained in industrial wastewater. It has been widely used in the field of organic wastewater treatment. However, the Fenton treatment technology for organic wastewater is limited to the acidic pH range, which greatly restricts the scope of application of the Fenton treatment technology for organic wastewater.

[0004] In addition, the technology of treating organic wastewater with microwaves, which has highly concentrated energy and high penetration characteristics, has also developed rapidly in recent years. When microwaves are used to treat organic wastewater, the electromagnetic field generated by microwaves not only causes the organic wastewater to produce more hydroxyl free radicals to enhance the Fenton treatment effect of organic matter, but also microwaves cause the organic matter to produce thermal effects, promoting the denaturation and decomposition of organic matter.

[0005] In view of the current technical bottlenecks of low acrylonitrile wastewater degradation rate and unsatisfactory chemical oxygen demand (COD) removal rate, the present invention has high acrylonitrile / chemical oxygen demand (COD) removal rate, wide pH treatment conditions and excellent reuse performance in the microwave-assisted Fenton treatment of acrylonitrile wastewater, effectively breaking through the development bottleneck of existing acrylonitrile-containing wastewater treatment technology. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the present invention provides a method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton. The catalyst prepared by the method has a high acrylonitrile / chemical oxygen demand (COD) removal rate, a wide pH treatment condition and excellent reusability.

[0007] The technical solution adopted by the present invention to solve its technical problem is:

[0008] The present invention provides a method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton treatment, comprising the following steps performed in sequence:

[0009] Step [1] forming a CuO(C4H8O)4 organic compound layer on the surface of the copper foam substrate;

[0010] Step [2] The CuO(C4H8O)4 organic compound layer on the surface of the copper foam is converted into Cu2O(C4H8O)2(C 14 H 12 O) 2 organic compound layer;

[0011] Step [3] In Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2.

[0012] Preferably, the step [1] specifically includes the following operations:

[0013] a1. Add copper chloride, aminosulfonic acid and pyridine to 2,3-butanediol and mix well to form a synthetic liquid;

[0014] a2. The copper foam sample is immersed in the synthetic solution, reacted at room temperature for 16-24 hours, and then the sample is taken out and immersed in ether for 5-12 minutes to remove by-products to obtain a copper foam with a CuO (C4H8O) 4 organic compound layer formed on the surface, which is recorded as intermediate A.

[0015] Preferably, in step a1, the concentration of copper chloride in the synthetic liquid is 540 g / L-580 g / L, the concentration of aminosulfonic acid is 130 g / L-160 g / L, and the concentration of pyridine is 30 mL / L-50 mL / L.

[0016] Preferably, in step a2, the weight of the copper foam immersed in each liter of the synthetic solution is 420-460 g.

[0017] Preferably, the specific operations of step [2] are:

[0018] b1. Add 1,2-diphenylethylene glycol, sodium borohydride and sodium methoxide to a mixed solvent of tetrahydrofuran and methanol to form a conversion replacement solution;

[0019] b2. Immerse the intermediate A in the conversion replacement solution and react at a constant temperature of 40-65°C for 4-6 hours to obtain a Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer of foam copper, recorded as intermediate B.

[0020] Preferably, the volume ratio of tetrahydrofuran to methanol in the mixed solvent is 0.8-1.2:1; the amount of 1,2-diphenylethylene glycol added per liter of the mixed solvent is 380g-420g, the amount of sodium borohydride added is 60g-90g, and the amount of sodium methoxide added is 40g-70g.

[0021] Preferably, the weight of the intermediate A immersed in each liter of the conversion replacement liquid is 250-280 g.

[0022] Preferably, the step [3] specifically includes the following operations:

[0023] c1. Adding lithium aluminum hydride, diphenyl glycolic acid, iron oxide and o-phenylenediamine to tetrahydrofuran and mixing to form a base liquid; adding sodium borohydride to methanol to form an additive liquid; adding a certain amount of the additive liquid to the base liquid and mixing to form an anchoring liquid;

[0024] c2. Immerse the intermediate B in the anchoring liquid and react at 50-70° C. for 12-18 hours to finally obtain the catalyst.

[0025] Preferably, in step c1, the amount of lithium aluminum hydride added to each liter of tetrahydrofuran is 60g-90g, the amount of diphenylhydroxyacetic acid added is 150g-190g, the amount of iron oxide added is 270g-300g, and the amount of o-phenylenediamine added is 120g-140g; the amount of sodium borohydride added to each liter of methanol is 140g-170g; and the volume ratio between the additive liquid and the base liquid in the anchoring liquid is 1-2:3-5.

[0026] Preferably, in step c2, the weight of the intermediate B immersed in each liter of the anchoring liquid is 340-380 g.

[0027] The positive effects of the present invention are as follows: the microwave-assisted Fenton catalyst for treating acrylonitrile wastewater prepared by the method according to the present invention (copper-based Cu2O(C4H8O)2(C 14 H 12 O)2 organic anchored ferrous complex hydride [Fe(C 14 H 13 O3N)6](BH4)2), its structural characteristics are: Cu2O(C4H8O)2(C 14 H 12 The structure of organic matter is tetrahedral, Cu2O is located in the center of the tetrahedron, isobutyraldehyde C4H8O and biphenylacetaldehyde C 14 H 12 O is located at the vertices of the regular tetrahedron; foam copper-based Cu2O(C4H8O)2(C 14 H 12 O)2 organic matter surface anchored ferrous complex hydride [Fe(C 14 H13 O3N)6](BH4)2 organic compounds, [Fe(C 14 H 13 O3N)6](BH4)2 is a ferrous ion at the center of the octahedron, and forms an octahedral structure [Fe(C 14 H 13 O3N)6] 2+ Coordinate ions and (BH4) - Based on the above structural characteristics, the highly concentrated and highly penetrating microwaves not only make the acrylonitrile-containing wastewater produce more hydroxyl radicals, but also make Cu2O(C4H8O)2(C 14 H 12 O)2 organic matter and acrylonitrile adsorption energy is reduced, making the carbon-carbon bond and carbon-nitrogen bond strength weaker and easier to break; ferrous complex hydride [Fe(C 14 H 13 O3N)6](BH4)2 provides ferrous ions and hydrogen peroxide to trigger the heterogeneous Fenton chain reaction. The hydroxyl radicals produced by the heterogeneous Fenton chain reaction have an oxidative degradation effect on acrylonitrile. In addition, microwaves produce a direct thermal effect on acrylonitrile, which significantly promotes the denaturation and decomposition of acrylonitrile.

[0028] The catalyst prepared according to the present invention has high acrylonitrile / chemical oxygen demand (COD) removal rate, wide pH treatment conditions and excellent reusability in microwave-assisted Fenton treatment of acrylonitrile-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the preparation process of the catalyst of the present invention;

[0030] Figure 2 It is a schematic diagram of the structure of CuO(C4H8O)4 of the present invention;

[0031] Figure 3 The Cu2O(C4H8O)2(C 14 H 12 O) Schematic diagram of the structure of 2;

[0032] Figure 4 The present invention is [Fe(C 14 H 13 Schematic diagram of the structure of O3N)6](BH4)2;

[0033] Figure 5a It is a comparison diagram of the relative concentration of benzonitrile residues in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention at a pH of 3;

[0034] Figure 5bIt is a comparison diagram of the relative concentration of benzonitrile residues in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention at a pH of 7;

[0035] Figure 5c It is a comparison diagram of the relative concentration of benzonitrile residues in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention at a pH of 10;

[0036] Figure 6 It is a comparison of COD removal rates of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention under different pH conditions;

[0037] Figure 7 It is a relationship diagram between the number of times of use and the removal rate of benzoacrylonitrile under specific conditions of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention;

[0038] Figure 8 It is a relationship diagram between the number of uses and the COD removal rate of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention under specific conditions. DETAILED DESCRIPTION

[0039] Reference Figure 1 The present invention provides a method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton treatment, comprising the following steps performed in sequence:

[0040] Step [1] forms a CuO(C4H8O)4 organic compound layer on the surface of the copper foam substrate, specifically comprising the following operations:

[0041] a1. Add copper chloride, sulfamic acid and pyridine to 2,3-butanediol and mix well to form a synthetic solution having a copper chloride concentration of 540g / L-580g / L, a sulfamic acid concentration of 130g / L-160g / L, and a pyridine concentration of 30mL / L-50mL / L;

[0042] a2. Immerse the copper foam sample in the synthetic solution (the weight of the copper foam immersed in each liter of the synthetic solution is 420-460 g), react at room temperature for 16-24 hours, take out the sample and immerse it in ether for 5-12 minutes to remove the by-products, and obtain a copper foam with a CuO(C4H8O)4 organic compound layer formed on the surface, which is recorded as intermediate A, wherein the structure of the CuO(C4H8O)4 is as follows Figure 2 shown.

[0043] Step [2] The CuO(C4H8O)4 organic compound layer on the surface of the copper foam is converted into Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer, the specific operation is:

[0044] b1. Add 1,2-diphenylethylene glycol, sodium borohydride and sodium methoxide to a mixed solvent of tetrahydrofuran and methanol (the amount of 1,2-diphenylethylene glycol added per liter of mixed solvent is 380g-420g, the amount of sodium borohydride added is 60g-90g, and the amount of sodium methoxide added is 40g-70g), and mix to form a conversion replacement liquid, wherein the volume ratio between tetrahydrofuran and methanol in the mixed solvent is 0.8 to 1.2: 1;

[0045] b2. Immerse the intermediate A in the conversion replacement solution (the weight of the intermediate A immersed in each liter of the conversion replacement solution is 250-280g), and react at a constant temperature of 40-65°C for 4-6 hours to convert the CuO(C4H8O)4 on the surface of the foam copper into Cu2O(C4H8O)2(C 14 H 12 O)2, and the surface is formed with Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer, denoted as intermediate B, wherein the Cu2O(C4H8O)2(C 14 H 12 O)2 structure as Figure 3 shown.

[0046] Step [3] In Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2, specifically including the following operations:

[0047] c1. Add lithium aluminum hydride, diphenyl glycolic acid, iron oxide and o-phenylenediamine to tetrahydrofuran (the amount of lithium aluminum hydride added per liter of tetrahydrofuran is 60g-90g, the amount of diphenyl glycolic acid added is 150g-190g, the amount of iron oxide added is 270g-300g, and the amount of o-phenylenediamine added is 120g-140g), and mix to form a base liquid; sodium borohydride is added to methanol (the amount of sodium borohydride added per liter of methanol is 140g-170g) to form an additive solution; add the additive solution to the base liquid in a volume ratio of 1 to 2:3 to 5, and mix to form an anchoring liquid;

[0048] c2. Immerse the intermediate B in the anchoring liquid (the weight of the intermediate B immersed in each liter of the anchoring liquid is 340-380 g), and react at 50-70 ° C for 12-18 hours to form Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H14 O2N)6](BH4)2, and finally obtain the catalyst (copper-based Cu2O(C4H8O)2(C 14 H 12 O)2 anchored [Fe(C 14 H 13 O3N)6](BH4)2 catalytic material), wherein the [Fe(C 14 H 13 O3N)6](BH4)2 structure is as follows Figure 4 shown.

[0049] The preferred embodiments of the present invention are described below by way of example.

[0050] Example 1

[0051] Preferred embodiment 1 of the present invention provides a method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton reaction, comprising the following steps performed in sequence:

[0052] Step [1] forms a CuO(C4H8O)4 organic compound layer on the surface of the copper foam substrate, specifically comprising the following operations:

[0053] a1. Add copper chloride, sulfamic acid and pyridine to 2,3-butanediol and mix well to form a synthetic solution having a copper chloride concentration of 550g / L, sulfamic acid concentration of 150g / L, and pyridine concentration of 40mL / L;

[0054] a2. The copper foam sample was immersed in the synthetic solution (the weight of the copper foam immersed in each liter of the synthetic solution was 460 g). After reacting at room temperature for 20 hours, the sample was taken out and immersed in ether for 10 minutes to remove by-products, and a copper foam with a CuO (C4H8O)4 organic compound layer formed on the surface was obtained, which was recorded as intermediate A.

[0055] Step [2] The CuO(C4H8O)4 organic compound layer on the surface of the copper foam is converted into Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer, the specific operation is:

[0056] b1. 1,2-diphenylethylene glycol, sodium borohydride and sodium methoxide were added to a mixed solvent of tetrahydrofuran and methanol (1,2-diphenylethylene glycol was added in an amount of 410 g, sodium borohydride was added in an amount of 80 g, and sodium methoxide was added in an amount of 70 g per liter of the mixed solvent) to form a conversion replacement solution, wherein the volume ratio of tetrahydrofuran to methanol in the mixed solvent was 1: 1;

[0057] b2. The intermediate A is immersed in the conversion replacement solution (the weight of the intermediate A immersed in each liter of the conversion replacement solution is 270g), and the reaction is carried out at a constant temperature of 60°C for 5 hours to convert the CuO(C4H8O)4 on the surface of the foam copper into Cu2O(C4H8O)2(C 14 H 12 O)2, and the surface is formed with Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer of foam copper, recorded as intermediate B.

[0058] Step [3] In Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2, specifically including the following operations:

[0059] c1. Add lithium aluminum hydride, diphenyl glycolic acid, iron oxide and o-phenylenediamine to tetrahydrofuran (80 g of lithium aluminum hydride, 180 g of diphenyl glycolic acid, 290 g of iron oxide and 130 g of o-phenylenediamine per liter of tetrahydrofuran) to form a base liquid; add sodium borohydride to methanol (160 g of sodium borohydride per liter of methanol) to form an additive liquid; add the additive liquid to the base liquid in a volume ratio of 2:5 to form an anchoring liquid;

[0060] c2. The intermediate B is immersed in the anchoring liquid (the weight of the intermediate B immersed in each liter of the anchoring liquid is 380 g), and reacted at 65 ° C for 17 hours to form Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2, and finally obtain the catalyst (copper-based Cu2O(C4H8O)2(C 14 H 12 O)2 anchored [Fe(C 14 H 13 O3N)6](BH4)2 catalytic material), recorded as Example 1.

[0061] Comparative Example 1

[0062] This comparative example 1 provides a copper-based Cu2O(C4H8O)2(C 14 H 12 The method for preparing an organic material comprises the following steps performed in sequence:

[0063] Step [1] forms a CuO(C4H8O)4 organic compound layer on the surface of the copper foam substrate, specifically comprising the following operations:

[0064] a1. Add copper chloride, sulfamic acid and pyridine to 2,3-butanediol and mix well to form a synthetic solution having a copper chloride concentration of 550g / L, a sulfamic acid concentration of 140g / L, and a pyridine concentration of 35mL / L;

[0065] a2. The copper foam sample was immersed in the synthetic solution (the weight of the copper foam immersed in each liter of the synthetic solution was 430 g). After reacting at room temperature for 18 hours, the sample was taken out and immersed in ether for 7 minutes to remove by-products, and a copper foam with a CuO (C4H8O)4 organic compound layer formed on the surface was obtained, which was recorded as intermediate A.

[0066] Step [2] The CuO(C4H8O)4 organic compound layer on the surface of the copper foam is converted into Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer, the specific operation is:

[0067] b1. 1,2-diphenylethylene glycol, sodium borohydride and sodium methoxide are added to a mixed solvent of tetrahydrofuran and methanol (1,2-diphenylethylene glycol is added in an amount of 400 g, sodium borohydride is added in an amount of 70 g, and sodium methoxide is added in an amount of 50 g per liter of the mixed solvent) to form a conversion replacement solution, wherein the volume ratio of tetrahydrofuran to methanol in the mixed solvent is 1.1: 1;

[0068] b2. The intermediate A is immersed in the conversion replacement solution (the weight of the intermediate A immersed in each liter of the conversion replacement solution is 260g), and the reaction is carried out at a constant temperature of 45°C for 5 hours to convert the CuO(C4H8O)4 on the surface of the foam copper into Cu2O(C4H8O)2(C 14 H 12 O)2, and the surface is formed with Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer of copper foam, that is, the copper foam base Cu2O(C4H8O)2(C 14 H 12 O)2 organic material, recorded as Comparative Example 1.

[0069] Comparative Example 2

[0070] This comparative example 2 provides a foam copper-based CuO (C4H8O) 4 organic anchored ferrous complex hydride [Fe (C 14 H 12The method for preparing an organic catalytic material comprises the following steps performed in sequence:

[0071] Step [1] forms a CuO(C4H8O)4 organic compound layer on the surface of the copper foam substrate, specifically comprising the following operations:

[0072] a1. Add copper chloride, sulfamic acid and pyridine to 2,3-butanediol and mix well to form a synthetic solution having a copper chloride concentration of 560g / L, a sulfamic acid concentration of 150g / L, and a pyridine concentration of 45mL / L;

[0073] a2. The copper foam sample was immersed in the synthetic solution (the weight of the copper foam immersed in each liter of the synthetic solution was 450 g). After reacting at room temperature for 20 hours, the sample was taken out and immersed in ether for 6 minutes to remove by-products, and a copper foam with a CuO (C4H8O)4 organic compound layer formed on the surface was obtained, which was recorded as intermediate A.

[0074] Step [2] Anchoring ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2, specifically including the following operations:

[0075] c1. Add lithium aluminum hydride, diphenyl glycolic acid, iron oxide and o-phenylenediamine to tetrahydrofuran (the amount of lithium aluminum hydride added per liter of tetrahydrofuran is 70 g, the amount of diphenyl glycolic acid added is 160 g, the amount of iron oxide added is 280 g, and the amount of o-phenylenediamine added is 130 g), and mix to form a base liquid; sodium borohydride is added to methanol (the amount of sodium borohydride added per liter of methanol is 150 g) to form an additive solution; the additive solution is added to the base liquid in a volume ratio of 2:3, and mixed to form an anchoring liquid;

[0076] c2. Immerse the intermediate A in the anchoring liquid (the weight of the intermediate A immersed in each liter of the anchoring liquid is 360 g), and react at 60°C for 16 hours to anchor the ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2, and finally obtain the foam copper-based Cu2O(C4H8O)4 organic anchored ferrous complex hydride [Fe(C 14 H 12 O2)6](BH4)2 organic catalytic material, recorded as Comparative Example 2.

[0077] In order to analyze the removal rate of acrylonitrile and COD, pH adaptability and reusability of microwave-assisted Fenton treatment of acrylonitrile-containing wastewater in Example 1, Comparative Example 1 and Comparative Example 2, an experimental solution with an acrylonitrile concentration of 400 mg / L was prepared using deionized water as a solvent as simulated acrylonitrile wastewater, and 500 ml of simulated acrylonitrile wastewater was treated with ultrasound-assisted Fenton at pH values ​​of 3, 7 and 10 for 80 minutes, wherein the microwave power was 400 W, the catalyst dosage was 20 g / L, and the hydrogen peroxide concentration was 20 mmol / L.

[0078] The residual benzonitrile in the simulated benzonitrile wastewater was analyzed by gas chromatography to calculate the removal rate of benzonitrile. The COD of the simulated benzonitrile wastewater was measured by a COD measuring instrument to calculate the COD removal rate. The corresponding residual benzonitrile relative concentration and COD removal rate results of Example 1, Comparative Example 1 and Comparative Example 2 under pH values ​​of 3, 7 and 10 are shown respectively. Figure 5a -c and Figure 6 As shown: the removal rate of residual benzonitrile in Example 1 at pH 3, pH 7 and pH 10 is more than 95%, and the removal rate of COD exceeds 90%; in contrast, the removal rates of benzonitrile in Comparative Example 1 and Comparative Example 2 at pH 3, pH 7 and pH 10 are no more than 40% and 60% respectively, and the highest COD removal rates are 44% and 58% respectively.

[0079] In order to analyze the repeated catalytic degradation performance of microwave-assisted Fenton treatment of acrylonitrile wastewater in Example 1, Comparative Example 1 and Comparative Example 2, 500 ml of simulated acrylonitrile wastewater was treated with microwave-assisted Fenton cycle at pH 3 for 80 minutes multiple times using Example 1, Comparative Example 1 and Comparative Example 2, respectively. The relationship between the number of times used and the acrylonitrile removal rate and COD removal rate is shown in the following table. Figure 7 , Figure 8 As shown: Example 1, which was repeatedly used 8 times under the condition of pH value of 3, can still achieve acrylonitrile and COD removal rates of more than 90% in the simulated acrylonitrile-containing wastewater. The removal rates of acrylonitrile and COD in comparative example 1 and comparative example 2, which were repeatedly used 8 times under the condition of pH value of 3, are less than 20% and 30%, respectively.

[0080] In summary, the catalyst prepared according to the present invention has high acrylonitrile / chemical oxygen demand (COD) removal rate, wide pH applicability and excellent reusability in the microwave-assisted Fenton treatment of acrylonitrile-containing wastewater.

[0081] To illustrate in further detail, three additional examples are provided below.

[0082] Example 2

[0083] Preferred embodiment 2 of the present invention provides a method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton reaction, comprising the following steps performed in sequence:

[0084] Step [1] forms a CuO(C4H8O)4 organic compound layer on the surface of the copper foam substrate, specifically comprising the following operations:

[0085] a1. Add copper chloride, sulfamic acid and pyridine to 2,3-butanediol and mix well to form a synthetic solution having a copper chloride concentration of 540g / L, sulfamic acid concentration of 130g / L, and pyridine concentration of 30mL / L;

[0086] a2. The copper foam sample was immersed in the synthetic solution (the weight of the copper foam immersed in each liter of the synthetic solution was 420 g). After reacting at room temperature for 16 hours, the sample was taken out and immersed in ether for 5 minutes to remove by-products, and a copper foam with a CuO (C4H8O)4 organic compound layer formed on the surface was obtained, which was recorded as intermediate A.

[0087] Step [2] The CuO(C4H8O)4 organic compound layer on the surface of the copper foam is converted into Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer, the specific operation is:

[0088] b1. 1,2-diphenylethylene glycol, sodium borohydride and sodium methoxide were added to a mixed solvent of tetrahydrofuran and methanol (1,2-diphenylethylene glycol was added in an amount of 420 g, sodium borohydride was added in an amount of 60 g, and sodium methoxide was added in an amount of 70 g per liter of the mixed solvent) to form a conversion replacement solution, wherein the volume ratio of tetrahydrofuran to methanol in the mixed solvent was 0.8: 1;

[0089] b2. The intermediate A is immersed in the conversion replacement solution (the weight of the intermediate A immersed in each liter of the conversion replacement solution is 280g), and the reaction is carried out at a constant temperature of 65°C for 4 hours to convert the CuO(C4H8O)4 on the surface of the foam copper into Cu2O(C4H8O)2(C 14 H 12 O)2, and the surface is formed with Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer of foam copper, recorded as intermediate B.

[0090] Step [3] In Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14O2N)6](BH4)2, specifically including the following operations:

[0091] c1. Add lithium aluminum hydride, diphenyl glycolic acid, iron oxide and o-phenylenediamine to tetrahydrofuran (the amount of lithium aluminum hydride added per liter of tetrahydrofuran is 60 g, the amount of diphenyl glycolic acid added is 190 g, the amount of iron oxide added is 270 g, and the amount of o-phenylenediamine added is 140 g), and mix to form a base liquid; sodium borohydride is added to methanol (the amount of sodium borohydride added per liter of methanol is 140 g) to form an additive solution; the additive solution is added to the base liquid in a volume ratio of 1:5, and mixed to form an anchoring liquid;

[0092] c2. Immerse the intermediate B in the anchoring liquid (the weight of the intermediate B immersed in each liter of the anchoring liquid is 340 g) and react at 50 ° C for 18 hours to form Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2, and finally obtain the catalyst (copper-based Cu2O(C4H8O)2(C 14 H 12 O)2 anchored [Fe(C 14 H 13 O3N)6](BH4)2 catalytic material).

[0093] Example 3

[0094] Preferred embodiment 3 of the present invention provides a method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton reaction, comprising the following steps performed in sequence:

[0095] Step [1] forms a CuO(C4H8O)4 organic compound layer on the surface of the copper foam substrate, specifically comprising the following operations:

[0096] a1. Add copper chloride, sulfamic acid and pyridine to 2,3-butanediol and mix well to form a synthetic solution having a copper chloride concentration of 580 g / L, a sulfamic acid concentration of 160 g / L, and a pyridine concentration of 50 mL / L;

[0097] a2. The copper foam sample was immersed in the synthetic solution (the weight of the copper foam immersed in each liter of the synthetic solution was 460 g). After reacting at room temperature for 24 hours, the sample was taken out and immersed in ether for 12 minutes to remove by-products, and a copper foam with a CuO (C4H8O)4 organic compound layer formed on the surface was obtained, which was recorded as intermediate A.

[0098] Step [2] The CuO(C4H8O)4 organic compound layer on the surface of the copper foam is converted into Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer, the specific operation is:

[0099] b1. 1,2-diphenylethylene glycol, sodium borohydride and sodium methoxide were added to a mixed solvent of tetrahydrofuran and methanol (1,2-diphenylethylene glycol was added in an amount of 380 g, sodium borohydride was added in an amount of 90 g, and sodium methoxide was added in an amount of 40 g per liter of the mixed solvent) to form a conversion replacement solution, wherein the volume ratio of tetrahydrofuran to methanol in the mixed solvent was 1.2: 1;

[0100] b2. The intermediate A is immersed in the conversion replacement solution (the weight of the intermediate A immersed in each liter of the conversion replacement solution is 252g), and the reaction is carried out at a constant temperature of 40°C for 6 hours to convert the CuO(C4H8O)4 on the surface of the foam copper into Cu2O(C4H8O)2(C 14 H 12 O)2, and the surface is formed with Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer of foam copper, recorded as intermediate B.

[0101] Step [3] In Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2, specifically including the following operations:

[0102] c1. Add lithium aluminum hydride, diphenyl glycolic acid, iron oxide and o-phenylenediamine to tetrahydrofuran (90 g of lithium aluminum hydride, 150 g of diphenyl glycolic acid, 300 g of iron oxide and 140 g of o-phenylenediamine per liter of tetrahydrofuran) to form a base liquid; add sodium borohydride to methanol (170 g of sodium borohydride per liter of methanol) to form an additive liquid; add the additive liquid to the base liquid in a volume ratio of 2:4 to form an anchoring liquid;

[0103] c2. Immerse the intermediate B in the anchoring liquid (the weight of the intermediate B immersed in each liter of the anchoring liquid is 340 g), and react at 70 ° C for 12 hours to form Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H14 O2N)6](BH4)2, and finally obtain the catalyst (copper-based Cu2O(C4H8O)2(C 14 H 12 O)2 anchored [Fe(C 14 H 13 O3N)6](BH4)2 catalytic material).

[0104] Example 4

[0105] Preferred embodiment 4 of the present invention provides a method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton reaction, comprising the following steps performed in sequence:

[0106] Step [1] forms a CuO(C4H8O)4 organic compound layer on the surface of the copper foam substrate, specifically comprising the following operations:

[0107] a1. Add copper chloride, sulfamic acid and pyridine to 2,3-butanediol and mix well to form a synthetic solution having a copper chloride concentration of 560g / L, sulfamic acid concentration of 145g / L, and pyridine concentration of 40mL / L;

[0108] a2. The copper foam sample was immersed in the synthetic solution (the weight of the copper foam immersed in each liter of the synthetic solution was 440 g). After reacting at room temperature for 20 hours, the sample was taken out and immersed in ether for 9 minutes to remove by-products, and a copper foam with a CuO (C4H8O)4 organic compound layer formed on the surface was obtained, which was recorded as intermediate A.

[0109] Step [2] The CuO(C4H8O)4 organic compound layer on the surface of the copper foam is converted into Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer, the specific operation is:

[0110] b1. 1,2-diphenylethylene glycol, sodium borohydride and sodium methoxide are added to a mixed solvent of tetrahydrofuran and methanol (1,2-diphenylethylene glycol is added in an amount of 400 g, sodium borohydride is added in an amount of 75 g, and sodium methoxide is added in an amount of 55 g per liter of the mixed solvent) to form a conversion replacement solution, wherein the volume ratio of tetrahydrofuran to methanol in the mixed solvent is 1: 1;

[0111] b2. The intermediate A is immersed in the conversion replacement solution (the weight of the intermediate A immersed in each liter of the conversion replacement solution is 265g), and the reaction is carried out at a constant temperature of 53°C for 5 hours to convert the CuO(C4H8O)4 on the surface of the foam copper into Cu2O(C4H8O)2(C 14 H 12O)2, and the surface is formed with Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer of foam copper, recorded as intermediate B.

[0112] Step [3] In Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2, specifically including the following operations:

[0113] c1. Add lithium aluminum hydride, diphenyl glycolic acid, iron oxide and o-phenylenediamine to tetrahydrofuran (the amount of lithium aluminum hydride added per liter of tetrahydrofuran is 75 g, the amount of diphenyl glycolic acid added is 170 g, the amount of iron oxide added is 285 g, and the amount of o-phenylenediamine added is 130 g), and mix to form a base liquid; sodium borohydride is added to methanol (the amount of sodium borohydride added per liter of methanol is 155 g) to form an additive liquid; the additive liquid is added to the base liquid in a volume ratio of 2:3, and mixed to form an anchoring liquid;

[0114] c2. The intermediate B is immersed in the anchoring liquid (the weight of the intermediate B immersed in each liter of the anchoring liquid is 360g), and reacted at 60°C for 15 hours to form Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2, and finally obtain the catalyst (copper-based Cu2O(C4H8O)2(C 14 H 12 O)2 anchored [Fe(C 14 H 13 O3N)6](BH4)2 catalytic material).

[0115] The above are only preferred embodiments of the present invention. It should be understood that the description of the above embodiments is only used to help understand the method and core ideas of the present invention, and is not used to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, etc. made within the ideas and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton reaction, characterized in that: It contains the following steps in order: Step [1] forming a CuO(C4H8O)4 organic compound layer on the surface of the copper foam substrate; Step [2] The CuO(C4H8O)4 organic compound layer on the surface of the copper foam is converted into Cu2O(C4H8O)2(C 14 H 12 O) 2 organic compound layer; Step [3] In Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer surface anchored ferrous complex hydride [Fe(C 14 H 14 O2N)6](BH4)2.

2. The method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton according to claim 1, characterized in that: The step [1] specifically includes the following operations: a1. Add copper chloride, aminosulfonic acid and pyridine to 2,3-butanediol and mix well to form a synthetic liquid; a2. The copper foam sample is immersed in the synthetic solution, reacted at room temperature for 16-24 hours, and then the sample is taken out and immersed in ether for 5-12 minutes to remove by-products to obtain a copper foam with a CuO (C4H8O) 4 organic compound layer formed on the surface, which is recorded as intermediate A.

3. The method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton according to claim 2, characterized in that: In step a1, the concentration of cupric chloride in the synthetic solution is 540 g / L-580 g / L, the concentration of aminosulfonic acid is 130 g / L-160 g / L, and the concentration of pyridine is 30 mL / L-50 mL / L.

4. The method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton according to claim 2, characterized in that: In step a2, the weight of the copper foam immersed in each liter of the synthetic solution is 420-460 g.

5. The method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton according to claim 1, characterized in that: The specific operations of step [2] are: b1. Add 1,2-diphenylethylene glycol, sodium borohydride and sodium methoxide to a mixed solvent of tetrahydrofuran and methanol to form a conversion replacement solution; b2. Immerse the intermediate A in the conversion replacement solution and react at a constant temperature of 40-65°C for 4-6 hours to obtain a Cu2O(C4H8O)2(C 14 H 12 O)2 organic compound layer of foam copper, recorded as intermediate B.

6. The method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton according to claim 5, characterized in that: The volume ratio of tetrahydrofuran to methanol in the mixed solvent is 0.8-1.2:1; the amount of 1,2-diphenylethylene glycol added per liter of the mixed solvent is 380g-420g, the amount of sodium borohydride added is 60g-90g, and the amount of sodium methoxide added is 40g-70g.

7. The method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton according to claim 5, characterized in that: The weight of the intermediate A immersed in each liter of the conversion replacement solution is 250-280 g.

8. The method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton according to claim 1, characterized in that: The step [3] specifically includes the following operations: c1. Adding lithium aluminum hydride, diphenyl glycolic acid, iron oxide and o-phenylenediamine to tetrahydrofuran and mixing to form a base liquid; adding sodium borohydride to methanol to form an additive liquid; adding a certain amount of the additive liquid to the base liquid and mixing to form an anchoring liquid; c2. Immerse the intermediate B in the anchoring liquid and react at 50-70° C. for 12-18 hours to finally obtain the catalyst.

9. The method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton according to claim 8, characterized in that: In step c1, the amount of lithium aluminum hydride added to each liter of tetrahydrofuran is 60g-90g, the amount of diphenylhydroxyacetic acid added is 150g-190g, the amount of iron oxide added is 270g-300g, and the amount of o-phenylenediamine added is 120g-140g; the amount of sodium borohydride added to each liter of methanol is 140g-170g; and the volume ratio between the additive liquid and the base liquid in the anchoring liquid is 1-2:3-5.

10. The method for preparing a catalyst for treating acrylonitrile wastewater by microwave-assisted Fenton according to claim 8, characterized in that: In step c2, the weight of the intermediate B immersed in each liter of the anchoring liquid is 340-380 g.