High-frequency pulse jet solution combustion preparation method of efficient nano oxygen evolution catalyst

Through the high-frequency double-pulse jet solution combustion method, the problems of uneven particles and agglomeration in the preparation of oxygen evolution catalysts are solved, the performance and purity of the catalyst are improved, the cost is reduced, and a green and sustainable preparation process is achieved.

CN118904401APending Publication Date: 2024-11-08JIANGSU YUNTIAN HYDROGEN ENERGY TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411055308.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing preparation methods for oxygen evolution catalysts, the reaction temperature and atmosphere are difficult to accurately control, resulting in uneven size and morphology of the catalyst particles, prone to agglomeration, and by-products, affecting the purity and performance of the catalyst.

Method used

The high-frequency double-pulse injection solution combustion method is adopted to accurately control the injection speed and frequency of the precursor and combustible solution through the injection device, and combine the conical nozzle and rotation technology to regulate the atmosphere and oxygen proportion in the combustion chamber to achieve uniform distribution of catalyst particles and High temperature combustion reduces agglomeration and improves purity.

Benefits of technology

It realizes precise control of the size of the catalyst particle, reduces agglomeration, improves the purity and performance of the catalyst, reduces production costs, complies with the principles of green chemistry, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904401A_ABST
    Figure CN118904401A_ABST
Patent Text Reader

Abstract

The invention relates to a high-frequency pulse jet solution combustion preparation method of an efficient nano oxygen evolution catalyst. The method comprises the following steps: preparing a metal salt precursor solution and a combustible solution, and controlling the injection of the solution at the frequency of 1-10 times per second through a high-frequency pulse injection device. And in the cylindrical combustion chamber, combustion is carried out through an ignition device, and thermal decomposition of the metal salt and crystallization of the catalyst are realized at high temperature. The nanometer oxygen evolution catalyst particles with the particle size of 30-100 nm are obtained, and the performance is optimized through annealing treatment at the temperature of 400-800 DEG C for 30-200 minutes. The temperature, pressure and oxygen content are monitored in real time in the combustion process. According to the method, the activity, selectivity and stability of the catalyst are improved, the particle aggregation phenomenon is reduced, the uniformity and consistency are improved, the water electrolysis hydrogen production efficiency is improved, and the development of a green energy technology is promoted. The method is efficient, simple, convenient, low in cost and environmentally friendly, and reliable technical support is provided for large-scale production of the high-performance oxygen evolution catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydrogen energy, and particularly relates to a method for preparing a high-efficiency nano oxygen evolution catalyst by high-frequency pulse jet solution combustion. Background Art

[0002] Water electrolysis technology is a renewable energy technology that decomposes water into hydrogen and oxygen through an electrochemical process. However, the oxygen evolution reaction (OER) in the water electrolysis process involves multiple electron transfers, and its reaction kinetics are relatively slow, resulting in a high overpotential, which restricts the overall efficiency of water electrolysis. Therefore, improving the performance of oxygen evolution reaction catalysts has become a technical problem that needs to be solved urgently.

[0003] In the current research on oxygen evolution catalysts, although precious metal catalysts (such as RuO2 and IrO2) show excellent catalytic activity, their high cost and scarcity limit their large-scale application. In recent years, non-precious metal catalysts (such as iron, cobalt, and nickel-based materials) have become a hot topic of research due to their abundant resources and low cost. However, during the preparation process, they face problems such as particle agglomeration, difficulty in controlling size and morphology, resulting in low catalytic efficiency.

[0004] The existing oxygen evolution catalyst preparation processes mainly include the following categories:

[0005] Co-precipitation method:

[0006] 1. Advantages: simple process and low cost.

[0007] 2. Disadvantages: It is difficult to control the particle size and morphology, which can easily lead to agglomeration of catalyst particles and affect catalytic performance.

[0008] Sol-Gel Method:

[0009] 1. Advantages: Uniform nanoparticles can be prepared, suitable for the preparation of a variety of metal oxides.

[0010] 2. Disadvantages: It requires high temperature treatment, high energy consumption, and is prone to cracks during drying and heat treatment.

[0011] Hydrothermal method:

[0012] 1. Advantages: High-purity catalysts can be prepared at relatively low temperatures, and the crystal structure is easy to control.

[0013] 2. Disadvantages: long reaction time, high equipment requirements, and difficult to mass produce.

[0014] Electrodeposition method:

[0015] 1. Advantages: It is easy to control the thickness and morphology of the deposited layer, suitable for the preparation of electrode materials.

[0016] 2. Disadvantages: The process is complicated, the electrolyte is easy to pollute the environment, and the deposition rate is slow.

[0017] However, existing non-precious metal catalysts have the following problems in the preparation process: Particle size and distribution are difficult to control: Traditional preparation methods make it difficult to accurately control the size and morphology of catalyst particles, resulting in low catalyst activity and selectivity. Particle agglomeration phenomenon: The prepared catalyst particles are prone to agglomeration, which reduces active sites and reduces catalytic efficiency. High energy consumption: Traditional methods usually require high temperature and high pressure conditions, which consumes a lot of energy and increases production costs. Environmental burden: Some preparation methods will produce a large amount of by-products and waste, causing certain pollution to the environment.

[0018] In order to reduce the cost of large-scale preparation of oxygen evolution catalysts and realize green preparation process, we need to focus on the method of preparing oxygen evolution catalysts at room temperature and pressure, mainly including:

[0019] Mechanical mixing method:

[0020] 1. Advantages: simple operation, no need for high temperature and high pressure equipment.

[0021] 2. Disadvantages: poor particle dispersion, easy to agglomerate, and low catalytic activity.

[0022] Chemical reduction method:

[0023] 1. Advantages: mild reaction conditions and simple operation.

[0024] 2. Disadvantages: Reducing agents can easily introduce impurities, affecting the purity and performance of the catalyst.

[0025] Solution combustion method:

[0026] 1. Advantages: Rapid reaction, the product is nanoparticles, suitable for large-scale production.

[0027] 2. Disadvantages: The reaction conditions are difficult to control, the particle size and morphology are uneven, and by-products are easily produced.

[0028] Among them, the solution combustion method is expected to be widely used in the large-scale preparation of oxygen evolution catalysts due to its advantages such as rapid reaction, simple method and nanoparticle products. However, it also has the following problems: (1) The reaction conditions are difficult to control accurately: During the solution combustion process, the temperature and atmosphere are difficult to control accurately, resulting in uneven catalyst particle size and morphology. (2) The particle agglomeration phenomenon is serious: During the combustion process, nanoparticles are prone to agglomeration, reducing the effective catalytic active sites. (3) There are many by-products: By-products are easily generated during the combustion process, affecting the purity and performance of the catalyst.

[0029] In view of the above problems, the present invention proposes a method for preparing an oxygen evolution catalyst by a high-frequency double-pulse jet solution combustion method, which is efficient, low-cost, green and pollution-free. Summary of the invention

[0030] The present invention aims to solve the problems existing in the existing technology for preparing oxygen evolution catalysts, such as the difficulty in accurately controlling the reaction temperature and atmosphere during solution combustion, which leads to uneven catalyst particle size and morphology, the easy agglomeration of nanoparticles during combustion, which reduces the effective catalytic active sites, and the easy generation of by-products during combustion, which affects the purity and performance of the catalyst. A high-frequency pulse jet solution combustion preparation method for an efficient nano oxygen evolution catalyst is proposed.

[0031] 1. Preparation method:

[0032] a) washing the porous catalyst support with 1M sodium hydroxide solution, 5wt.% dilute hydrochloric acid and ultrapure water in sequence through a spray device to remove surface impurities and roughen the support surface;

[0033] b) preparing a metal salt precursor solution and a combustible solution;

[0034] c) using a double pulse spray device to spray the precursor solution and the combustible solution onto the surface of the porous catalyst in the combustion chamber;

[0035] d) In the combustion chamber, a metal salt precursor solution is burned at high temperature on the surface of the carrier by an ignition device, and the metal salt is thermally decomposed to obtain a porous monolithic catalyst; the combustion chamber is equipped with a temperature sensor, a pressure sensor and a gas analyzer to monitor and control the combustion process; high-frequency pulses and high-temperature environments are used as screening mechanisms to screen catalyst particles with stable structures;

[0036] e) Control the atmosphere and oxygen ratio in the combustion chamber and regulate the combustion process;

[0037] f) annealing the prepared catalyst;

[0038] g) Rinse the catalyst surface with ultrapure water through a spray device to ensure rapid cooling of the catalyst and prevent agglomeration.

[0039] Beneficial effects of the present invention:

[0040] Control of particle size and distribution: Through high-frequency double-pulse injection technology, the injection speed and frequency of the precursor solution and the combustible solution can be accurately controlled, the solution combustion reaction time and the catalyst particle growth rate can be adjusted, and the size of the catalyst particles can be stabilized within the range of 30-100nm. The combination of conical nozzle and rotation technology increases the dispersion and atomization uniformity of the solution, ensures that the solution can be evenly distributed during the injection process, effectively prevents the accumulation of the solution in a fixed position, and thus achieves uniform distribution of particles.

[0041] Reduce particle agglomeration: In the cylindrical combustion chamber, the temperature of the catalyst carrier surface can be controlled within the range of 300-1400°C by controlling the proportion of oxygen and the proportion of combustible solution. The controllable catalyst preparation temperature and pulse injection technology help to screen out catalyst particles with stable structure and strong binding force, reduce particle agglomeration, and ensure the uniformity and consistency of catalyst particles.

[0042] Improve catalyst purity: In view of the problem of by-product impurities in the current solution combustion method when burning in the air, a combustion chamber is designed to control the ratio of oxygen and nitrogen, and there are no other impurities in the gas, thereby improving the purity of the catalyst.

[0043] Green and pollution-free: This method complies with the principles of green chemistry and reduces waste generation and the burden on the environment by optimizing the combustion process and post-processing steps.

[0044] Through the above improvements, the process of the present invention not only solves the problems existing in the existing solution combustion technology for preparing oxygen evolution catalysts, but also improves the performance of the oxygen evolution catalysts, reduces production costs, and promotes the green and sustainable development of the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 For example 1, the catalyst scanning electron microscope (SEM) image,

[0046] Figure 2 Take the LSV performance curve of catalyst oxygen evolution reaction in Example 1 as an example.

[0047] Figure 3 Take the LSV performance curve of catalyst oxygen evolution reaction in Example 2 as an example.

[0048] Figure 4 Take the LSV performance curve of catalyst oxygen evolution reaction in Example 3 as an example.

[0049] Figure 5 Take the LSV performance curve of catalyst 4 during oxygen evolution reaction as example. DETAILED DESCRIPTION

[0050] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0051] Example 1

[0052] First, prepare the precursor metal solution: the concentration of ferric chloride is 100, 120, 140, 160, and 180 mM, respectively, and a mixture of 90% ethanol and 10% deionized water by volume is used as the combustible solution. Then, use a double pulse injection device with a nozzle diameter of 100 μm, set the pulse frequency to 7 times / second, and accurately control the injection of the precursor solution and the combustible solution. In the cylindrical combustion chamber, the oxygen ratio is controlled to 25%, and thermal decomposition is achieved at a high temperature of 500 ° C. Finally, the product is annealed at 600 ° C for 120 minutes to obtain an oxygen evolution catalyst. The morphology and structure of the catalyst are shown in the attached Figure 1 , OER performance curve is attached Figure 2 .from Figure 1 It can be seen that many spherical or nearly spherical particles of different sizes are closely gathered together to form a honeycomb-like structure. This structure is usually beneficial to increase the surface area of ​​the catalyst, thereby enhancing its catalytic activity. In addition, the catalyst particles have good dispersibility and porosity, which can increase the chance of contact between the reactants and the catalyst, thereby improving the catalytic efficiency.

[0053] Example 2

[0054] Prepare the precursor solution: ferric chloride (180mM) is mixed with cobalt chloride (180mM), manganese chloride (120mM), sodium molybdate (100mM), sodium tungstate (140mM), and nickel chloride (120mM). A mixture of 70% ethylene glycol and 30% deionized water by volume is used as the combustible solution. Then, a double-pulse injection device with a nozzle diameter of 100μm is used, and the pulse frequency is set to 6 times / second to accurately control the injection of the precursor solution and the combustible solution. In the cylindrical combustion chamber, the oxygen ratio is controlled to 30%, and thermal decomposition is achieved at a high temperature of 600℃. Finally, the product is annealed at 700℃ for 120 minutes. The LSV performance curve of the oxygen evolution reaction is attached. Figure 3 .

[0055] Example 3

[0056] Prepare a metal precursor solution: ferric chloride (152.5mM), sodium molybdate (130mM), graphite powder (120mM), boric acid (170mM), and add 4wt.% trisodium citrate as a binder. Methanol, ethanol, ethylene glycol and 50% methanol-ethanol, methanol-ethylene glycol, ethanol-ethylene glycol were used as combustible solutions respectively. Use a double pulse injection device with a nozzle diameter of 100μm, and set the pulse frequency to 5 times / second. In a cylindrical combustion chamber, the oxygen ratio is controlled to 35%, and thermal decomposition is achieved at a high temperature of 700℃. The product is annealed at 750℃ for 100 minutes to obtain an oxygen evolution catalyst. The LSV performance curve of the oxygen evolution reaction is attached. Figure 4 .

[0057] Example 4

[0058] Prepare a metal precursor solution: sodium molybdate (130mM), graphite powder (120mM), urea (175mM) and boric acid (170mM), and add 2wt.% trisodium citrate as a binder. Use a mixture of 90% ethanol and 10% deionized water by volume as a combustible solution. Then, use a double-pulse injection device with a nozzle diameter of 100μm, set the pulse frequency to 4 times / second, and accurately control the injection of the precursor solution and the combustible solution. In the cylindrical combustion chamber, the oxygen ratio is controlled to 25%, and thermal decomposition is achieved at a high temperature of 500°C. Finally, the product is annealed at 650°C for 120 minutes to obtain oxygen evolution catalyst particles. The LSV performance curve of the oxygen evolution reaction is attached. Figure 5 .

[0059] The above describes the basic principle and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. Preparation method of high-frequency pulse jet solution combustion of efficient nano oxygen evolution catalyst, It is characterized in that The preparation steps are as follows: a) washing the porous catalyst support with 1M sodium hydroxide solution, 5wt.% dilute hydrochloric acid and ultrapure water in sequence through a spray device to remove surface impurities and roughen the support surface; b) preparing a metal salt precursor solution and a combustible solution; c) using a double pulse spray device to spray the precursor solution and the combustible solution onto the surface of the porous catalyst in the combustion chamber; d) in the combustion chamber, a metal salt precursor solution is burned at high temperature on the surface of the carrier by an ignition device, and the metal salt is thermally decomposed to obtain a porous monolithic catalyst; e) Control the atmosphere and oxygen ratio in the combustion chamber and regulate the combustion process; f) annealing the prepared catalyst; g) Rinse the catalyst surface with ultrapure water through a spray device to ensure rapid cooling of the catalyst and prevent agglomeration.

2. The high-frequency pulse jet solution combustion preparation method of the high-efficiency nano oxygen evolution catalyst according to claim 1, It is characterized in that The spray device is a double pulse nozzle, which controls the spraying of the metal salt precursor solution and the combustible solution respectively. The nozzle in the spray device rotates at a constant speed, and the rotation speed ranges from 200 to 1000 rpm. The pulse frequency of the liquid sprayed by the spray device is 1 to 10 times per second. The diameter of the nozzle in the pulse spray device is preferably 50 to 200 μm to optimize the atomization effect of the solution, and the nozzle is conical to increase the dispersion and atomization uniformity of the solution.

3. The high-frequency pulse jet solution combustion preparation method of the high-efficiency nano oxygen evolution catalyst according to claim 1, It is characterized in that The precursor solution is a metal salt of an active component of an oxygen evolution catalyst, a mixture of one or more of ruthenium chloride, iridium trichloride, ferric chloride, cobalt chloride, nickel chloride, manganese chloride, sodium molybdate, and sodium tungstate in any proportion, and its concentration is in the range of 10-200 mM.

4. The method for preparing a high-efficiency nano-oxygen evolution catalyst by high-frequency pulse jet solution combustion according to claim 1, It is characterized in that The precursor solution also includes a thickener, and the thickener is preferably hexachlorobenzene or yellow soap powder, and the concentration is preferably 1-5% (weight percentage).

5. The method for preparing a high-efficiency nano-oxygen evolution catalyst by high-frequency pulse jet solution combustion according to claim 1, It is characterized in that The flammable solution is one of methanol, ethanol, ethylene glycol and water or a mixture of the three alcohols in any proportion, wherein the proportion of water contained in the mixture is 0-50%.

6. The method for preparing a high-efficiency nano-oxygen evolution catalyst by high-frequency pulse jet solution combustion according to claim 1, It is characterized in that The combustion chamber is cylindrical, with a diameter of 200 mm and a length of 500 mm. The proportion of oxygen is between 10-40%. The high-temperature environment formed by burning the solution is between 300-1400° C., and the combustion reaction time is 1-60 minutes.

7. The method for preparing a high-efficiency nano-oxygen evolution catalyst by high-frequency pulse jet solution combustion according to claim 1, It is characterized in that The annealing temperature is 400-800° C. and the time is 30-200 minutes.

8. The method for preparing a high-efficiency nano-oxygen evolution catalyst by high-frequency pulse jet solution combustion according to claim 1, It is characterized in that The combustion chamber is equipped with a temperature sensor, a pressure sensor and a gas analyzer for monitoring and controlling the combustion process.

9. The method for preparing a high-efficiency nano-oxygen evolution catalyst by high-frequency pulse jet solution combustion according to claim 1, It is characterized in that High-frequency pulses and high-temperature environments are used as screening mechanisms to screen catalyst particles with stable structures.

Citation Information

Patent Citations

  • Pulse type spray evaporation flame synthesis method and device

    CN112717848A

  • Ni-FeOx / FeNi3 / NF composite electrocatalyst as well as preparation method and application thereof

    CN114990616A

  • Pulse jet system and method

    WO2013033039A1