Surface coating processing technology applied to steel structure in total immersion area

By etching and coating the surface of marine steel structures with an epoxy resin mixture and amino-modified POSS treatment, the problems of easy paint peeling and poor antifouling effect of marine steel structures are solved, achieving high adhesion and durable anti-corrosion effect.

CN118904690APending Publication Date: 2024-11-08CHINA UNIV OF PETROLEUM (BEIJING)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410961263.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing marine steel structure coatings have problems such as easy peeling and short-lasting antifouling effect in terms of corrosion and fouling prevention. Moreover, the requirements for coatings in marine environments are more stringent, and they must not blister or break under long-term scouring.

Method used

A steel surface is etched using a mixed solution of silica and HF under plasma equipment, followed by coating with an epoxy resin mixture and undergoing an amino-modified POSS treatment to form a nano-sized porous structure to enhance adhesion and impart hydrophobic and oleophobic properties.

Benefits of technology

It improves the adhesion between the coating and the substrate, enhances corrosion and fouling resistance, and exhibits superior durability and hydrophobic properties, making it suitable for corrosion protection of fully immersed oil and gas pipelines and ships.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904690A_ABST
    Figure CN118904690A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of steel structure surface treatment, and particularly discloses a steel structure surface coating processing technology applied to a total immersion zone, and the specific operation flow is as follows: firstly coating a layer of mixed solution of silicon dioxide and HF on the steel surface, then etching the surface through plasma treatment, and enabling the silicon dioxide to permeate to a certain extent; then surface cleaning is conducted, and the etched stainless steel surface is coated with epoxy resin; and finally, dipping the amino-modified POSS on the surface, and heating at a certain temperature. According to the anticorrosive coating for the steel structure and the preparation method, the corrosion problem of the steel structure in the marine total immersion area can be effectively solved, the surface of the steel structure is etched through the HF solution and the silicon dioxide under the plasma condition, so that a nano-sized hole structure is machined in the surface of the steel structure, and the nano-sized hole structure is conveniently permeated and combined with coating macromolecules; and the effect is more reliable than that of using an adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel structure surface treatment, and in particular relates to a surface coating processing technology for a full immersion zone steel structure. Background Art

[0002] With the continuous expansion of the scale of marine development, a large number of metal and alloy materials are used in the marine environment. The corrosion and fouling of metal materials in the ocean have always been a major problem that plagues the development of the marine economy. For the fouling caused by the attachment of marine organisms and the electrochemical corrosion caused by hydrogen ions, chloride ions and oxygen in the marine environment to ships and offshore facilities, the most common method to prevent and control such corrosion is to apply a protective coating system on the metal surface for protection.

[0003] These coatings are divided into organic coatings and inorganic coatings. They are effective means to protect steel structures from corrosion. However, as surface coatings for marine steel structures, the standards should be stricter than those for inland steel structure coatings. They have higher requirements for the surface treatment of steel structures and must not cause bubbling or damage to the surface coating of steel structures under long-term erosion by seawater.

[0004] At present, these coatings are mainly used for anti-corrosion and anti-fouling, but they all have the problems of easy falling off and short-lasting anti-fouling effect. Summary of the invention

[0005] The purpose of the present invention is to provide a surface coating processing technology for steel structures in full immersion zone to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A coating process for the surface of a steel structure in a full immersion zone, S1, firstly coating the steel surface with a mixed solution of silicon dioxide and HF, and then etching the steel surface by plasma treatment, and causing a certain penetration of silicon dioxide;

[0008] S2, then cleaning the surface of the steel structure, and then applying the epoxy resin mixture to the etched stainless steel surface;

[0009] S3. Finally, the amino-modified POSS is impregnated on the surface and reacted at a temperature of 70-80°C for 3-4 hours.

[0010] Preferably, the mixed solution of silicon dioxide and HF involved in S1 is mainly operated by coating a 40% hydrofluoric acid solution containing 7.5% silicon dioxide on the surface of the stainless steel, etching for 1 to 5 minutes at room temperature, and the working power of the etcher is 500W.

[0011] Preferably, the epoxy resin mixture in S2 comprises: 2.5% carbon nanotubes (diameter 20-30 nm, length 10-30 nm), 2.5% nano Al2O3 powder (diameter 150-200 nm), and 95% epoxy resin, and the preparation method of the epoxy resin mixture comprises the following steps:

[0012] Use the shear stirring and dispersion of the high-speed shear instrument to pour 95 parts of the epoxy resin solution into a container, divide the weighed nano-alumina powder into three parts relatively evenly, and before putting it into the shear instrument for stirring, pour in a part of non-nano-alumina powder and stir it with a stirring rod for 1-2 minutes to avoid uneven agglomeration during subsequent shear stirring, and then carry out shear stirring for a total of 30 minutes, adding a part of nano-alumina powder every 10 minutes; then carry out shear stirring for a total of 60 minutes for the carbon nanotubes that are relatively evenly divided into three parts, and add a part every 20 minutes.

[0013] The epoxy resin mixed liquid after shearing and stirring is ultrasonically dispersed. After one hour of ultrasonic dispersion, the epoxy resin mixed liquid is carefully and steadily taken out. If no bubbles are observed in the mixed liquid and no powder particles are precipitated at the bottom of the beaker, it is well dispersed.

[0014] Preferably, the amino-modified POSS in S3 is NH2-POSS.

[0015] Preferably, the metal surface etching in S1 adopts NI E-4000 (A) fully automatic IBE ion beam etcher, with RF power of 500 W, flow rate of 50 cm3 / s, etching rate of 0.8 μm / min, and etching time of 30 s to 1 min.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. In the anti-corrosion coating for steel structure and its preparation method, the surface of the steel structure is etched by HF solution and silicon dioxide under plasma conditions, so that a nano-sized hole structure is processed on the surface, which is convenient for mutual penetration and combination with the coating polymer to enhance the bonding force between the two, and the effect is more reliable than using an adhesive.

[0018] 2. The anti-corrosion coating for steel structure is compounded with amino-containing POSS and epoxy resin, so that the coating has hydrophobic and oleophobic properties, and can prevent fouling and adhesion of other substances in seawater. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a surface image of the steel structure after etching in the present invention;

[0020] Figure 2Schematic diagram of the contact angle of the steel structure coated with the anti-corrosion layer obtained in Examples 1-4 of the present invention and Comparative Examples 1-2. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Embodiment 1:

[0023] ① Apply a 40% hydrofluoric acid solution containing 7.5% silicon dioxide to the stainless steel surface, and etch for 3 minutes at room temperature. The working power of the etcher is 500W; ② After the surface is cleaned, a mixed component of 2.5% carbon nanotubes (diameter 25nm, length 30nm), 2.5% nano-Al2O3 powder (diameter 200nm), and 95% epoxy resin is evenly applied to the etched stainless steel structure surface; ③ The amino-modified POSS solution is infiltrated into the stainless steel structure surface obtained in step ②, and the reaction is carried out at a temperature of 75°C for 3.5h.

[0024] Embodiment 2:

[0025] ① Apply a 40% hydrofluoric acid solution containing 7.5% silicon dioxide to the stainless steel surface, etch for 5 minutes at room temperature, and the working power of the etcher is 500W; ② After the surface is cleaned, a mixed component of 2.5% carbon nanotubes (diameter 20nm, length 10nm), 2.5% nano Al2O3 powder (diameter 150nm), and 95% epoxy resin is evenly applied to the etched stainless steel structure surface; ③ The amino-modified POSS solution is infiltrated into the stainless steel structure surface obtained in step ②, and reacted at a temperature of 70°C for 4h.

[0026] Embodiment three:

[0027] ① Apply a 40% hydrofluoric acid solution containing 7.5% silicon dioxide to the stainless steel surface, etch for 1 min at room temperature, and the working power of the etcher is 500 W; ② After the surface is cleaned, a mixed component of 2.5% carbon nanotubes (diameter 20nm, length 25nm), 2.5% nano-Al2O3 powder (diameter 180nm), and 95% epoxy resin is evenly applied to the etched stainless steel structure surface; ③ The amino-modified POSS solution is infiltrated into the stainless steel structure surface obtained in step ②, and reacted at a temperature of 80°C for 3h.

[0028] Embodiment 4:

[0029] ① Apply a 40% hydrofluoric acid solution containing 7.5% silicon dioxide to the stainless steel surface, etch for 2 minutes at room temperature, and the working power of the etcher is 500W; ② After the surface is cleaned, a mixed component of 2.5% carbon nanotubes (diameter 20nm, length 20nm), 2.5% nano-Al2O3 powder (diameter 200nm), and 95% epoxy resin is evenly applied to the etched stainless steel structure surface; ③ The amino-modified POSS solution is infiltrated into the stainless steel structure surface obtained in step ②, and reacted at a temperature of 70°C for 3h.

[0030] Comparative Example 1

[0031] ① Apply a 40% hydrofluoric acid solution containing 7.5% silicon dioxide to the stainless steel surface, etch for 2 minutes at room temperature, and the working power of the etcher is 500W; ② After the surface is cleaned, a mixed component of 2.5% carbon nanotubes (diameter 20nm, length 20nm), 2.5% nano Al2O3 powder (diameter 200nm), and 95% epoxy resin is evenly applied to the etched stainless steel structure surface; react at a temperature of 70°C for 3h.

[0032] Comparative Example 2

[0033] ① After cleaning the steel structure surface, a mixture of 2.5% carbon nanotubes (diameter 20nm, length 20nm), 2.5% nano-Al2O3 powder (diameter 200nm), and 95% epoxy resin is evenly coated on the etched stainless steel structure surface; ③ The amino-modified POSS solution is infiltrated into the stainless steel structure surface obtained in step ②, and reacted at a temperature of 70°C for 3h.

[0034] Tests and Results:

[0035] (1) Test of the bonding strength between substrate and coating:

[0036] Refer to GB / T 9286-1998 Paint and varnish, cross-cut test of paint film. Paint film adhesion refers to the degree of firmness of the paint film combined with the surface of the coated object. Adhesion is one of the important indicators of the physical and mechanical properties of the coating. Through this inspection, the composition of the coating can be tested.

[0037] Especially whether the use of resin is reasonable. Use a blade with a cutter gap of 1mm. Apply the sample to the sample and pull it parallel to the sample for 3 to 4cm. There are six cuts, which should cut through the paint film to the substrate; then use the same method to make six cuts perpendicular to the former; this will form many small squares. Then apply tape and quickly pull it apart, and use visual or magnifying glass to compare and grade against the standard. The grading standard is described as:

[0038] Level 0: The cutting edge is completely smooth, without any falling off;

[0039] Level 1: A small amount of coating falls off at the intersection, and the affected area cannot be significantly greater than 5%;

[0040] Level 2: The coating falls off at the fork or along the edge of the cut, affecting an area of ​​5% to 15%;

[0041] Level 3: The coating partially or completely falls off along the cutting edge in a large area, and the affected cross-cut area is 15% to 35%;

[0042] Level 4: The entire edge is peeled off, and some grids are partially or completely peeled off. The affected area is 35% to 65%, and the degree of peeling exceeds Level 4.

[0043] (2) Salt water resistance test

[0044] Refer to GB 10834-1989 Determination of salt water resistance of ship paint. Use refined edible salt and distilled water to prepare a 3.5 mass% salt water solution. The test salt water solution is replaced every 3 days. The temperature is maintained at 25°C. After the temperature is kept constant, hang the sample so that three-quarters of it is immersed in the salt water solution. After the test, take the sample out of the test tank, rinse the sample carefully with tap water, gently dry it with filter paper, and check and record whether there is discoloration, blistering, wrinkling, shedding, rusting, etc.

[0045] Table 1 Contact angle, salt water resistance and binding force of different samples

[0046]

[0047]

[0048] According to the above table, compared with the steel structure with an anti-corrosion layer prepared by Examples 1-4 and the steel structure with an anti-corrosion layer prepared by Comparative Examples 1-2, the anti-corrosion steel structure prepared by the process used in the examples has better bonding between the anti-corrosion layer and the base steel structure, and has a large contact angle, has a hydrophobic effect, and is more resistant to salt water corrosion. In addition, although the contact angle of Comparative Example 2 is greater than 90° and has a hydrophobic effect, due to the weak bonding between the epoxy resin and the steel surface, a slight shedding phenomenon also occurs. The surface etching treatment of the steel structure can indeed increase the bonding between the epoxy resin and the steel and the silica infiltrated therein. Therefore, the anti-corrosion coating and the anti-corrosion coating obtained by the preparation process of the present invention exhibit extremely high corrosion resistance and superior durability. It can be widely used in the anti-corrosion of oil and gas pipelines and ships in full immersion areas.

[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A coating process for steel structure surface in full immersion zone, characterized in that: The following steps are involved: S1. First, a layer of mixed solution of silicon dioxide and HF is coated on the steel surface, and then the steel surface is etched by plasma treatment, and silicon dioxide is infiltrated to a certain extent; S2, then cleaning the surface of the steel structure, and then applying the epoxy resin mixture to the etched stainless steel surface; S3. Finally, the amino-modified POSS is impregnated on the surface and reacted at a temperature of 70-80°C for 3-4 hours.

2. The coating processing technology for full immersion zone steel structure according to claim 1 is characterized in that: The mixed solution of silicon dioxide and HF involved in S1 is mainly operated by coating a 40% hydrofluoric acid solution containing 7.5% silicon dioxide on the surface of stainless steel, etching for 1 to 5 minutes at room temperature, and the working power of the etcher is 500W.

3. The coating processing technology for full immersion zone steel structure according to claim 1 is characterized in that: The epoxy resin mixture in S2 comprises: 2.5% carbon nanotubes (diameter 20-30nm, length 10-30nm), 2.5% nano Al2O3 powder (diameter 150-200nm), and 95% epoxy resin. The preparation method of the epoxy resin mixture comprises the following steps: Use the shear stirring and dispersion of the high-speed shear instrument to pour 95 parts of the epoxy resin solution into a container, divide the weighed nano-alumina powder into three parts relatively evenly, and before putting it into the shear instrument for stirring, pour in a part of non-nano-alumina powder and stir it with a stirring rod for 1-2 minutes to avoid uneven agglomeration during subsequent shear stirring, and then carry out shear stirring for a total of 30 minutes, adding a part of nano-alumina powder every 10 minutes; then carry out shear stirring for a total of 60 minutes for the carbon nanotubes that are relatively evenly divided into three parts, and add a part every 20 minutes. The epoxy resin mixed liquid after shearing and stirring is ultrasonically dispersed. After one hour of ultrasonic dispersion, the epoxy resin mixed liquid is taken out. If no bubbles are observed in the mixed liquid and no powder particles are precipitated at the bottom of the beaker, the dispersion is good.

4. The surface coating processing technology for steel structure in full immersion zone according to claim 1 is characterized in that: The amino-modified POSS in S3 is NH2-POSS.

5. The surface coating processing technology for steel structure in full immersion zone according to claim 1 is characterized in that: The metal surface in S1 is etched using a NIE-4000(A) fully automatic IBE ion beam etcher with a radio frequency power of 500 W, a flow rate of 50 cm3 / s, an etching rate of 0.8 μm / min, and an etching time of 30 s to 1 min.