Hot continuous rolling process for avoiding layering of carbon steel-stainless steel composite plate

By controlling the heating temperature difference and adopting a hot continuous rolling process with air-through mode and medium-guided rolling, the problem of layering of carbon steel-stainless steel composite plates in the vacuum hot-rolling composite process is solved, and the material yield and mechanical properties are improved, thereby avoiding the Layering and waste roll loss of rolled parts.

CN118904908APending Publication Date: 2024-11-08SHANDONG SHIHENG SPECIAL STEEL GROUP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411167874.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Carbon steel-stainless steel composite plates are prone to post-rolling and layering in vacuum hot-rolling composite process, resulting in rolling and breaking of rolled parts or scrap steel, mainly due to the uneven material deformation and different thermal expansion coefficients.

Method used

A thermal continuous rolling process that avoids layering of carbon steel-stainless steel composite plates is adopted. By controlling the temperature difference of heating temperature, the air-through mode and medium-guided rolling are adopted to ensure the stable combination of carbon steel and stainless steel layer, and reduce vertical roll-to-combination. The side pressure of the plate increases the yield rate.

Benefits of technology

The layering problem of carbon steel-stainless steel composite board is effectively avoided, the loss of scrap coils is reduced, the yield is improved, and the heating quality and mechanical properties of composite boards are ensured.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of rolling compounding, in particular to a hot continuous rolling process for avoiding layering of a carbon steel-stainless steel composite board, which comprises the steps of raw material treatment, heating, rough rolling, finish rolling and coiling. During heating, the head temperature-middle temperature of the composite plate blank is 1t; 30 DEG C, tail temperature-middle temperature lt; 30 DEG C; during rough rolling, the rolling reduction of the first pass is 22%-25%, a rough rolling vertical roller adopts an air passing mode, the side pressure amount is 0 during vertical roller rolling, and the rough rolling vertical roller is only centered and guided; during finish rolling, the small finish rolling vertical roll adopts an idle mode, the side pressure amount is zero during rolling of the vertical roll, and the small finish rolling vertical roll only performs centering guiding. Through temperature difference control over the head, the middle and the tail of the composite plate blank during heating, the plasticity of the carbon steel-stainless steel blank is improved, the cracking probability of the head and the tail is reduced, vertical roll air passing is adopted for rough rolling and finish rolling, and the layering problem of a carbon steel layer and a stainless steel layer in the rolling process of the carbon steel-stainless steel composite plate is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rolling composite, and in particular to a hot continuous rolling process for avoiding delamination of a carbon steel-stainless steel composite plate. Background Art

[0002] Carbon steel-stainless steel composite plate is usually made of stainless steel as the surface material and ordinary carbon steel as the base material, which is composited by a specific process and is widely used in industries such as petroleum, chemical industry, salt industry, water conservancy and electricity. As a resource-saving product, carbon steel-stainless steel composite plate combines the good corrosion resistance of stainless steel and the excellent mechanical properties of carbon steel, which can reduce the consumption of precious metals, greatly reduce the project cost, and achieve a perfect combination of low cost and high performance. It has good economic benefits, market competitive advantages and social and economic benefits, and is an important direction for the development of steel products in the future.

[0003] The production processes of stainless steel composite plates generally include explosive composite process, vacuum hot rolling composite process, and cold rolling composite process. At present, the composite method of carbon steel-stainless steel composite plates generally adopts vacuum hot rolling composite process, that is, carbon steel and stainless steel are sealed and welded, and then heated and rolled under normal pressure after vacuuming. This method avoids the oxidation of the interface during the hot rolling composite process and has a low production cost, but the bonding effect of carbon steel and stainless steel is prone to be poor during the rolling process, and the rolling extrusion causes vacuum leakage, resulting in post-rolling stratification, which causes the rolled piece to be broken or scrapped. The main reason for post-rolling stratification is that the base layer and the composite layer of the composite plate are composed of two materials with different deformation resistance and thermal expansion coefficients. During normal hot rolling, the uneven deformation of the two materials causes serious stratification of warping or buckling, which affects the normal rolling of the rolling mill and causes failures. Summary of the invention

[0004] Aiming at the problem that carbon steel-stainless steel composite plates are prone to delamination after rolling in a vacuum hot rolling composite process, the present invention provides a hot continuous rolling process for avoiding delamination of carbon steel-stainless steel composite plates.

[0005] The technical solution of the present invention is as follows: A hot rolling process for avoiding delamination of a carbon steel-stainless steel composite plate, the steps of which include raw material processing, heating, rough rolling, finish rolling and coiling; During heating, the head temperature - middle temperature of the composite slab is <30°C, and the tail temperature - middle temperature is <30°C; during rough rolling, the first pass reduction is 22%-25%, the rough rolling vertical rolls adopt the empty passing mode, the side pressure during vertical roll rolling is 0, and the rough rolling vertical rolls are only guided to the center; during finishing rolling, the finishing small vertical rolls adopt the empty passing mode, the side pressure during vertical roll rolling is 0, and the finishing small vertical rolls are only guided to the center.

[0006] Furthermore, the total thickness of the carbon steel-stainless steel composite plate is 156 mm to 176 mm, and the thickness ratio of the carbon steel to the stainless steel is 10 to 11:1.

[0007] Furthermore, four stages of heating are performed during heating, including heating stage one, heating stage two, heating stage three and soaking stage, and the time in the furnace for the four stages of heating is controlled within 30-35 minutes.

[0008] Furthermore, the temperature of the first heating section is 800-1000°C, the temperature of the second heating section is 1020-1150°C, the temperature of the third heating section is 1200-1230°C, the upper ambient temperature of the ambient heat section is 1210-1230°C, and the lower ambient temperature of the ambient heat section is 1230-1250°C.

[0009] Furthermore, the lower soaking temperature of the soaking section is controlled to be 20° C. higher than the upper soaking temperature of the soaking section.

[0010] Furthermore, the rough rolling is performed for a total of 5 passes, with a large rough rolling reduction, and the total rough rolling reduction is not less than 80%.

[0011] Furthermore, the finishing rolling outlet temperature is 860-900°C.

[0012] Furthermore, the coiling temperature is 680-720°C.

[0013] The beneficial effects of the present invention are: The present invention provides a hot rolling process for avoiding stratification of carbon steel-stainless steel composite plates. During heating, the carbon steel-stainless steel composite plates require that the heating temperature is not too high, and in particular, the temperature difference between the head, middle and tail of the composite plate blank is ensured, the head temperature-middle temperature <30°C, and the tail temperature-middle temperature <30°C. By controlling the temperature, the plasticity of the carbon steel-stainless steel blank is improved, the probability of head and tail cracking is reduced, and the heating quality of the composite plate blank is ensured. Moreover, increasing the first pass reduction of rough rolling is conducive to the diffusion of bonding layer atoms to form a stable bonding layer, which is conducive to improving the interface assembly effect. Both rough rolling and fine rolling use vertical rollers passing empty and free widening, which avoids the vertical rollers squeezing the side of the carbon steel-stainless steel composite plate during the rolling process, eliminates the stratification problem of the carbon steel layer and the stainless steel layer during the rolling of the carbon steel-stainless steel composite plate, reduces the loss of waste coils, and improves the yield rate. DETAILED DESCRIPTION

[0014] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0015] Example 1 A hot rolling process for avoiding delamination of a carbon steel-stainless steel composite plate comprises the following steps: (1) Raw material processing: A carbon steel-stainless steel composite plate with a thickness of 176 mm (the thickness ratio of carbon steel to stainless steel is 10:1) was prepared.

[0016] The carbon steel is Q235B carbon steel, and the element composition by weight percentage is: C 0.19%, Si 0.25%, Mn 0.35%, P0.04%, S 0.04%, and the balance is Fe and inevitable impurities. The stainless steel is 304 stainless steel, and the element composition by weight percentage is: C 0.03%, Si 0.35%, Mn 0.52%, P 0.03%, S 0.002%, Ni 8.05%, Cr 18.25%, and the balance is Fe and inevitable impurities.

[0017] (2) Heating: After carbon steel and stainless steel are composited by conventional vacuum hot rolling composite process, the composite slab is sent to the heating furnace. The furnace time of heating stage 1, heating stage 2, heating stage 3 and soaking stage is controlled within 30 min. The temperature of heating stage 1 is 800°C, the temperature of heating stage 2 is 1020°C, the temperature of heating stage 3 is 1200°C, the upper soaking temperature of soaking stage is 1210°C, the lower soaking temperature of soaking stage is 1230°C, and the steel tapping temperature is 1130°C. During heating, the head temperature - middle temperature of the composite slab is 20°C, and the tail temperature - middle temperature is 20°C.

[0018] (3) Rough rolling: Rough rolling is performed with a large reduction for a total of 5 passes. The reduction in the first pass is 25%, and the total reduction in rough rolling is 82%. The rough rolling vertical rolls adopt the empty passing mode. The side pressure during vertical roll rolling is 0 (no side pressure is distributed), and only the center guide is used.

[0019] Centering guidance only means that the vertical rollers act as the guide at the inlet of the rolling mill, guiding the composite slab to bite into the roughing mill and ensuring the centering of the rolling center line.

[0020] (4) Finishing rolling: The finishing rolling small vertical roller adopts the empty passing mode. The side pressure during vertical roller rolling is 0 (no side pressure is distributed), only the center guide is used, and the finishing rolling outlet temperature is 860℃.

[0021] Centering guidance only means that the vertical rollers act as the guide at the inlet of the rolling mill, guiding the composite slab to bite into the finishing mill to ensure the centering of the rolling center line.

[0022] (5) Coiling: The coiling temperature is 680°C.

[0023] During the hot rolling process, there is no delamination of the carbon steel layer and the stainless steel layer, and there is no shedding phenomenon. The carbon steel-stainless steel composite plate is qualified for rolling. The mechanical properties of the carbon steel-stainless steel composite plate are similar to those of the base Q235B, with an upper yield strength of 320MPa, a tensile strength of 400MPa, and an elongation of 36%.

[0024] Example 2 A hot rolling process for avoiding delamination of a carbon steel-stainless steel composite plate comprises the following steps: (1) Raw material processing: A carbon steel-stainless steel composite plate with a thickness of 156 mm (the thickness ratio of carbon steel to stainless steel is 11:1) was prepared.

[0025] The carbon steel is Q235B carbon steel, and the element composition by weight percentage is: C 0.19%, Si 0.25%, Mn 0.35%, P0.04%, S 0.04%, and the balance is Fe and inevitable impurities. The stainless steel is 304 stainless steel, and the element composition by weight percentage is: C 0.03%, Si 0.35%, Mn 0.52%, P 0.03%, S 0.002%, Ni 8.05%, Cr 18.25%, and the balance is Fe and inevitable impurities.

[0026] (2) Heating: After carbon steel and stainless steel are composited by conventional vacuum hot rolling composite process, the composite slab is sent to the heating furnace. The furnace time of heating stage 1, heating stage 2, heating stage 3 and soaking stage is controlled at 35 min. The temperature of heating stage 1 is 1000°C, the temperature of heating stage 2 is 1150°C, the temperature of heating stage 3 is 1230°C, the upper soaking temperature of soaking stage is 1230°C, the lower soaking temperature of soaking stage is 1250°C, and the steel tapping temperature is 1180°C. During heating, the head temperature - middle temperature of the composite slab is 28°C, and the tail temperature - middle temperature is 28°C.

[0027] (3) Rough rolling: Rough rolling is performed with high reduction for a total of 5 passes. The reduction in the first pass is 22%, and the total reduction in rough rolling is 80%. The rough rolling vertical rolls adopt the empty passing mode. The side pressure during vertical roll rolling is 0 (no side pressure is distributed), and only the center guide is used.

[0028] (4) Finishing rolling: The finishing rolling small vertical roller adopts the empty passing mode. The side pressure during vertical roller rolling is 0 (no side pressure is distributed), only the center guide is used, and the finishing rolling outlet temperature is 900℃.

[0029] (5) Coiling: The coiling temperature is 720°C.

[0030] During the hot rolling process, the carbon steel layer and the stainless steel layer of the carbon steel-stainless steel composite plate have no delamination phenomenon such as warping or buckling, and there is no falling off phenomenon. The carbon steel-stainless steel composite plate is rolled to be qualified.

[0031] Comparative Example 1 The difference from Example 1 is that (2) during heating, the tail temperature-middle temperature is 35°C.

[0032] During the hot rolling process of carbon steel-stainless steel composite plates, as the temperature drop at the tail of the intermediate billet intensifies, the rolling load at the tail increases sharply, causing the tail to be rolled and delaminated.

[0033] Comparative Example 2 The difference from Example 1 is that (4) a small vertical roll strip side pressure is used in the finishing rolling, and the side pressure is 20 mm.

[0034] During the hot rolling process, the carbon steel-stainless steel composite plate is extruded by the vertical rollers, which causes cracks at the junction of the carbon steel layer and the stainless steel layer of the composite plate, resulting in delamination. The extrusion of the vertical rollers also aggravates the turtle back of the composite plate, affecting the plate shape quality of the composite plate.

[0035] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.

Claims

1. A hot rolling process for avoiding delamination of carbon steel-stainless steel composite plates, characterized in that: The steps include raw material handling, heating, rough rolling, finishing rolling and coiling; During heating, the head temperature - middle temperature of the composite slab is <30°C, and the tail temperature - middle temperature is <30°C; during rough rolling, the first pass reduction is 22%-25%, the rough rolling vertical rolls adopt the empty passing mode, the side pressure during vertical roll rolling is 0, and the rough rolling vertical rolls are only guided to the center; during finishing rolling, the finishing small vertical rolls adopt the empty passing mode, the side pressure during vertical roll rolling is 0, and the finishing small vertical rolls are only guided to the center.

2. A hot rolling process for avoiding delamination of carbon steel-stainless steel composite plates as claimed in claim 1, characterized in that: The total thickness of the carbon steel-stainless steel composite plate is 156mm-176mm, and the thickness ratio of carbon steel to stainless steel is 10-11:

1.

3. A hot rolling process for avoiding delamination of carbon steel-stainless steel composite plates as claimed in claim 1, characterized in that: Four stages of heating are carried out during heating, including heating stage one, heating stage two, heating stage three and soaking stage. The time in the furnace for the four stages of heating is controlled within 30-35 minutes.

4. A hot rolling process for avoiding delamination of carbon steel-stainless steel composite plates as claimed in claim 3, characterized in that: The temperature of the first heating section is 800-1000°C, the temperature of the second heating section is 1020-1150°C, the temperature of the third heating section is 1200-1230°C, the upper ambient temperature of the ambient section is 1210-1230°C, and the lower ambient temperature of the ambient section is 1230-1250°C.

5. A hot rolling process for avoiding delamination of carbon steel-stainless steel composite plates as claimed in claim 4, characterized in that: The lower ambient temperature of the ambient section is controlled to be 20°C higher than the upper ambient temperature of the ambient section.

6. A hot rolling process for avoiding delamination of carbon steel-stainless steel composite plates as claimed in claim 1, characterized in that: The rough rolling is carried out for 5 passes in total, with a large rough rolling reduction, and the total rough rolling reduction is not less than 80%.

7. A hot rolling process for avoiding delamination of carbon steel-stainless steel composite plates as claimed in claim 1, characterized in that: The finishing rolling outlet temperature is 860-900℃.

8. A hot rolling process for avoiding delamination of carbon steel-stainless steel composite plates as claimed in claim 1, characterized in that: The coiling temperature is 680-720℃.

Citation Information

Patent Citations

  • Manufacturing method for producing single face stainless steel composite plate by adopting hot continuous rolling set

    CN102553919A

  • Manufacturing method for producing double-sided stainless steel composite board by hot continuous rolling unit

    CN107661900A

  • Single-sided composite plate coiling hot rolling and production process thereof

    CN113500095A

  • Production process of single-sided stainless steel composite plate of hot continuous rolling unit

    CN113522973A

  • Hot continuous rolling strip steel rolling production process for corrosion-resistant stainless steel and carbon steel composite plate

    CN116371916A