High-yield and high-elongation copper-aluminum-copper composite board as well as preparation process and application thereof
Through the method of controlling the quantity and multiple rolling and annealing, the existing copper-aluminum-copper composite plate production methods are solved, and copper-aluminum-copper composite plates with high yield strength and elongation are prepared to meet the mechanical properties Requirements have broadened the scope of application.
Patent Information
- Application Number
- CN202411192915.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing production methods of copper-aluminum-copper composite panels have problems such as high cost, low efficiency, complex process and product thickness limitations, which are difficult to meet application scenarios with high mechanical performance requirements.
The copper-aluminum-copper composite plate with high yield strength and high elongation is prepared by single-pass large down pressure rough rolling and multiple-pass small down pressure fine rolling, combined with annealing treatment. Ensure that the thickness of the copper-aluminum-copper composite plate is between 0.1mm-0.2mm and meet the mechanical performance requirements.
The high yield strength and elongation of copper-aluminum-copper composite boards are achieved, the forming process is simplified, the production efficiency is improved, the application range is broadened, and the cost is reduced.
Smart Images

Figure CN118904910A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal plate processing, and specifically relates to a copper-aluminum-copper composite plate with high yield and high elongation, and a preparation process and application thereof. Background Art
[0002] The copper / aluminum / copper three-layer structure composite plate has the advantages of copper's high electrical and thermal conductivity, low contact resistance, and aluminum's light weight. At the same time, it avoids the shortcomings of copper's shortage of resources and high prices, while aluminum's poor wear resistance and corrosion resistance. It has broad application prospects in the fields of electronics, electricity, electrical appliances, metallurgy, machinery, automobiles, and daily necessities.
[0003] The copper / aluminum / copper three-layer structure composite sheet utilizes the good electrical and thermal conductivity of copper and the light weight and low cost of aluminum or aluminum alloy. The aluminum layer is the internal matrix and bears the main mechanical properties, and the outer copper layer plays a conductive role. It has the characteristics of light weight, good electrical and thermal conductivity, etc.
[0004] At present, there are many methods for producing metal composite materials, which can be roughly divided into two categories: solid-solid composite method and liquid-solid composite method. Solid-solid composite method includes rolling composite, explosive composite, extrusion-drawing composite, welding method, etc., and liquid-solid composite method includes core filling continuous casting, double crystallizer continuous casting, etc. Among them, the rolling composite method is the easiest method to achieve large-scale industrial production due to its low cost and simple processing technology. Compared with the rolling composite method, other methods have problems such as high cost, low efficiency, time consumption, long process route, and a large number of product defects.
[0005] In the prior art, the Chinese invention patent application publication number is CN102205346 A, which is a method for preparing a copper-aluminum-copper composite plate, which is to set two copper alloys with surface cleaning pretreatment vertically opposite to each other, pour the molten aluminum liquid between the two copper alloys to obtain an alloy blank, heat treat the alloy blank, and then roll to obtain a copper-aluminum-copper three-layer composite plate, and finally post-roll the copper-aluminum-copper three-layer composite plate to obtain a copper-aluminum-copper composite plate. It solves the problem of low copper / aluminum interface bonding strength caused by easy oxidation of the copper surface, and the interface bonding strength of the copper / aluminum composite plate can be increased by nearly 3 times compared with direct flat butt rolling. However, this technology requires melting the aluminum ingot and keeping the aluminum liquid in a high temperature state during casting. This process not only has high requirements for process and equipment, but also has huge costs. In addition, the thickness of the copper-aluminum-copper three-layer composite plate prepared by this method will be very thick, which limits its application scenarios. The manufacturing method of the copper-aluminum-copper three-layer composite plate with the Chinese invention patent application publication number CN1408485A uses ordinary electrolytic copper as raw material, inserts it into the gaps on both sides of the molybdenum ingot in the graphite mold, and then puts the mold into a heating furnace using hydrogen or other reducing gases as protective gas to heat it, and then processes it through heat preservation, hot rolling, heat treatment, etc. However, this technology requires to be carried out under vacuum or atmosphere protection, and the preparation process is complicated, which is not conducive to industrial production. Summary of the invention
[0006] In view of this, the purpose of the present invention is to propose a copper-aluminum-copper composite plate with high yield and high elongation. During the preparation process, the thickness of the copper-aluminum-copper composite plate can be made thin enough by controlling the amount of multiple rolling, and at the same time, it has high yield strength and elongation, which can meet the occasions with high mechanical property requirements and broaden the application range of the copper-aluminum-copper composite plate.
[0007] A copper-aluminum-copper composite plate with high yield and high elongation of the present invention comprises upper and lower copper layers and an aluminum layer in the middle layer, wherein the copper layer is a pure copper layer, and the thickness of the upper and lower copper layers is equal. Since the copper-aluminum-copper composite plate needs to utilize the high electrical and thermal conductivity of copper, the purity of copper is preferably between 99.9% and 99.99%. Preferably, in order to ensure the mechanical properties of the copper-aluminum-copper composite plate, the thickness of the aluminum layer exceeds 80%.
[0008] The mechanical properties of copper-aluminum-copper composite plates should also be considered during the application process. Selecting an aluminum alloy base with good mechanical properties and good formability is an effective way. In the present invention, the aluminum alloy selects a high-strength aluminum alloy that meets the following requirements: a tensile strength of more than 290MPa, a yield strength of more than 150MPa, and an elongation of more than 24%. Based on the good mechanical properties of 5456 aluminum alloy, using 5456 aluminum alloy as an intermediate layer of copper-aluminum-copper composite plates is a new attempt to improve the mechanical properties of composite plates. In the copper / aluminum / copper three-layer structure, the middle 5456 layer will provide matrix strength, and the copper surface layers on both sides will play a role in electrical conductivity and heat conduction. In addition, 5B59 aluminum alloy and 5056 aluminum alloy also have the potential to be used as an intermediate layer.
[0009] In a preferred embodiment, the thickness of the pure copper layer is preferably 0.2mm-0.4mm, and the thickness of the aluminum alloy layer is 3.3mm-6mm. The copper-aluminum-copper is prepared by a composite process with a large amount of downward pressure, and then annealed to eliminate the internal stress of the copper. Subsequently, a copper-aluminum-copper composite plate with a thickness of 0.1mm-0.2mm is obtained through multiple rolling passes, and then annealed to make the copper-aluminum-copper plate have a higher yield strength and elongation. When the thickness is 0.1mm-0.2mm, it still has the good mechanical properties of high-strength aluminum alloy. Annealing is a heat treatment process that improves the performance of the material by heating the material to a certain temperature and keeping it for a period of time and then slowly cooling it. The main purposes of annealing include releasing stress, increasing the ductility and toughness of the material, and producing a special microstructure.
[0010] The copper-aluminum-copper composite plate of the present invention is prepared by a rolling process, and the process steps include: material pretreatment, rolling and compounding, and annealing. The key to the process steps is a rolling method of a single-pass high-reduction rate rough rolling combined with a multi-pass low-reduction rate finishing rolling of the copper-aluminum-copper three-layer material, and the required mechanical properties are obtained by adjusting the subsequent annealing process.
[0011] Specifically, a preparation process of a high-yield and high-elongation copper-aluminum-copper composite plate of the present invention comprises the following steps:
[0012] S1. First, pre-treat the surface of the metal sheet
[0013] (1) Roughening removes the oxide film on the surface of the metal sheet to expose the fresh metal inside;
[0014] (2) Punching holes at the head of the metal sheet to facilitate riveting and fixing of the metal sheet;
[0015] (3) Ultrasonic cleaning for 10 minutes to remove stains and dust on the surface of the metal plate;
[0016] S2. The metal plates are stacked in the order of copper, aluminum and copper, the heads of the metal plates are fixed by riveting, and single-pass large-reduction rough rolling is performed at room temperature, the reduction rate is 70%, and the rough rolling speed is 1m / min-2m / min. After rolling, the surface oil is cleaned and dried;
[0017] S3. After rough rolling, the copper-aluminum-copper composite plate needs to be diffused annealed at a temperature of 400°C-500°C for 10min-60min to eliminate the internal stress of the copper and restore the composite plate to the O state;
[0018] S4, subsequently, the copper-aluminum-copper composite plate is rolled to 0.1 mm-0.2 mm by multiple passes of finishing rolling, each with a reduction rate of 15% to 21%; the number of finishing rolling passes varies according to the change of the reduction rate each time;
[0019] S5. The copper-aluminum-copper composite plate after fine rolling is further heat-treated, heated to 250°C-300°C, and kept warm for 5min-30min to improve the mechanical properties of the copper-aluminum-copper composite plate and obtain a copper-aluminum-copper plate with better performance.
[0020] The present invention selects metal sheets with good mechanical properties, first performs rough rolling and annealing with a single large reduction, and then performs fine rolling and subsequent annealing processes to obtain copper-aluminum-copper thin plates with higher yield strength and elongation. By selecting aluminum alloys with good mechanical properties, such as one of 5456 aluminum alloy, 5B59 aluminum alloy, and 5056 aluminum alloy; controlling the thickness of the pure copper layer to be 0.2mm-0.4mm, and the thickness of the aluminum alloy layer to be 3.3mm-6mm; using the aluminum alloy with good mechanical properties as the main matrix, the copper-aluminum-copper composite plate can still have good mechanical properties when the thickness is very thin. First, the laminated copper-aluminum-copper three-layer metal sheet is punched and riveted to fix one end of the three-layer material to maintain stability during the rolling process; the copper-aluminum-copper metal sheet is also pre-treated before lamination, including ultrasonic cleaning and roughening treatment. After the surface treatment of the material is completed, the copper-aluminum-copper composite is completed at room temperature through a large-pressure composite rolling process, the rolling speed is 1m / min-2m / min, the reduction rate is 70%, and a copper-aluminum-copper composite plate with good interface bonding is obtained. After the rough rolling composite, diffusion annealing treatment is required, the annealing temperature is 400℃-500℃, preferably 460℃, the annealing time is 10min-60min, preferably 30min, to eliminate the internal stress of the copper and restore the composite plate to the O state. Subsequently, the copper-aluminum-copper composite plate is rolled to 0.1mm-0.2mm through multiple rolling passes, and then stress relief annealing is performed, heated to 250℃-300℃, and kept warm for 5min-30min, preferably 10min-20min, to obtain a copper-aluminum-copper composite plate with good performance. The reduction rate is controlled at 15% to 21% each time.
[0021] The advantages of the present invention are: through controlled multiple rolling and compounding, the preparation of a copper-aluminum-copper composite plate with good bonding is achieved, the forming process is simple, the production efficiency is high, the yield strength and elongation of the copper-aluminum-copper composite plate are high, and the high electrical conductivity and high thermal conductivity characteristics of the copper-aluminum material itself are taken into account, and it can be used in occasions with higher mechanical property requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Schematic diagram of the bonding interface of the copper-aluminum-copper composite plate of Example 1. DETAILED DESCRIPTION
[0023] In order to make the technical personnel in the field understand the present invention more clearly and intuitively, the present invention will be further described below in conjunction with the accompanying drawings. The experimental methods without specific conditions in the following examples are selected according to conventional methods and conditions, or according to the product instructions.
[0024] Example 1
[0025] The materials selected in this embodiment are 5456 aluminum alloy and pure copper. Pure copper has good electrical and thermal conductivity, while 5456 aluminum alloy has good yield strength and elongation, and bears the main mechanical properties of the copper-aluminum-copper composite plate. The thickness of the selected pure copper layer is 0.2±0.02mm, and the thickness of the aluminum alloy layer is 3.3±0.1mm, both of which are in O state.
[0026] When preparing the copper-aluminum-copper composite plate, the surface of the metal plate needs to be pretreated first. The metal plate is first roughened, and then the three layers of copper-aluminum-copper metal plates are stacked together for punching and riveting to form a whole. Finally, the stacked three layers of metal plates are ultrasonically cleaned, and the cleaning time is preferably 10 minutes. The roughening treatment is because the oxide film on the surface of the aluminum alloy plate and the pure copper plate will hinder the rolling composite and reduce the interface bonding strength, so the roughening treatment is required. The oxide layer on the surface of the aluminum alloy plate and the pure copper plate is polished off by the roughening treatment to leak out the fresh metal. After the roughening treatment is completed, ultrasonic cleaning can be performed to carry out single-pass large-pressure composite rolling at room temperature, with a pressure of 70% and a rolling speed of 2m / min. When the composite rolling is completed, the thickness of the copper-aluminum-copper composite plate should be about 1.11mm. The composite copper-aluminum-copper composite plate needs to be diffused annealed, with an annealing temperature of 460°C and an annealing time of 30min to eliminate the internal stress of the copper-aluminum-copper composite plate and restore the composite plate to the O state. After diffusion annealing, clean the metal sheet to remove oil stains. In order to increase the composite strength of copper-aluminum-copper composites, achieve metallurgical bonding between each other, and also to further reduce the thickness of the composite plate, this embodiment performs 9 passes of precision rolling on the copper-aluminum-copper composite plate that has completed preliminary rolling. The thickness deformation each time is: 1.11mm (deformation 0.22) → 0.89mm (deformation 0.18) → 0.71mm (deformation 0.14) → 0.57mm (deformation 0.11) → 0.46mm (deformation 0.09) → 0.37mm (deformation 0.07) → 0.30mm (deformation 0.06) → 0.24mm (deformation 0.05) → 0.19mm (deformation 0.03) → 0.16mm. The finished product obtained after multiple rolling passes was sent to the annealing furnace for annealing to adjust the mechanical properties of the copper-aluminum-copper composite plate. The temperature of the annealing furnace was set to 200°C, 250°C, 280°C, 300°C, 310°C, 320°C, 360°C, 400°C, and the annealing time was 10 minutes. The results are shown in Table 1.
[0027] Table 1 Mechanical properties of copper-aluminum-copper composite panels under different treatment conditions
[0028]
[0029]
[0030] 1. Mechanical properties of copper-aluminum-copper composite panels
[0031] This embodiment uses a 5 series aluminum alloy with good mechanical properties (tensile strength of more than 290 MPa, yield strength of more than 150 MPa, and elongation of more than 24%) as a matrix. Therefore, the 5 series aluminum alloy provides a basic guarantee for the basic mechanical properties of the composite metal plate, and the process method is a key factor affecting the mechanical properties of the metal composite plate.
[0032] 2. Temperature and time of finished product annealing
[0033] The final annealing of the finished product is the key to adjusting the mechanical properties of the copper-aluminum-copper composite plate. High temperature or long time will lead to excessive grain growth and decreased mechanical properties; low temperature or short time will lead to incomplete annealing, too high yield strength, and low elongation. Taking into account the need to control production efficiency in actual production, the annealing time needs to be as short as possible. This embodiment mainly examines the effect of temperature on the mechanical properties of the copper-aluminum-copper composite plate. The preferred temperature is 250℃~300℃, which can ensure that the mechanical properties of the 0.16mm copper-aluminum-copper composite plate have sufficiently large advantages when the heating time is 10min.
[0034] 3. Pressing amount and rolling speed of composite rolling
[0035] The copper-aluminum-copper three-layer laminate is initially composited by the initial rolling with a large downward pressure and the control of the rolling speed, and then a good composite interface is obtained by multiple finishing rolling. Figure 1 shown.
[0036] The advantages of the present invention over the step-by-step composite rolling process are:
[0037] 1. The process steps are reduced, the forming process is simple, and the rolling amount can be controlled properly, which has high production efficiency, low cost and less time consumption;
[0038] 2. Through large-pressure rolling composite, copper-aluminum-copper three-layer composite is achieved. Combined with multiple passes of finishing rolling, the single finishing rolling reduction rate is controlled between 15% and 21% to obtain a good bonding interface.
[0039] 3. The copper-aluminum-copper composite plate has a yield strength of nearly 150MPa and an elongation of 14% when the thickness is 0.16mm. The composite plate also takes into account the high electrical conductivity and high thermal conductivity of the copper-aluminum material itself, which greatly increases the application field of the copper-aluminum-copper composite plate.
[0040] In the present invention, the purpose of using a large downward pressure in rough rolling is to allow the copper-aluminum-copper composite plate to have a preliminary composite state. Therefore, the key to obtaining good interface bonding strength is to improve the interface bonding strength of the copper plate and the aluminum plate through multiple passes of finishing rolling at the residual temperature after annealing after rough rolling.
[0041] In addition, in actual production, the more times of finishing rolling, the lower the production efficiency will be. Therefore, when the performance requirements of the prepared product are met, the number of finishing rolling should be shortened as much as possible for cost considerations.
[0042] Comparative Example 1
[0043] The difference between this embodiment and embodiment 1 is that after rough rolling and annealing, the number of finishing rolling is changed to 10 times to obtain a 0.16 mm copper-aluminum-copper composite plate.
[0044] The specific preparation method of the copper-aluminum-copper composite plate of this comparative example is as follows:
[0045] The thickness of the copper-aluminum-copper composite plate should be about 1.11 mm after composite rolling using the rough rolling method of Example 1. The composite copper-aluminum-copper composite plate needs to be subjected to diffusion annealing treatment at an annealing temperature of 460° C. for 30 minutes to eliminate the internal stress of the copper-aluminum-copper composite plate and restore the composite plate to an O state. After diffusion annealing, the plate is cleaned to remove oil stains.
[0046] This comparative example performs 8 passes of precision rolling on the copper-aluminum-copper composite plate that has completed preliminary rolling. The thickness deformation each time is: 1.11mm (deformation 0.13) → 0.98mm (deformation 0.12) → 0.86mm (deformation 0.12) → 0.74mm (deformation 0.11) → 0.63mm (deformation 0.11) → 0.52mm (deformation 0.10) → 0.42mm (deformation 0.08) → 0.34mm (deformation 0.08) → 0.26mm (deformation 0.06) → 0.20mm (deformation 0.04) → 0.16mm. The finished product obtained after multiple passes of rolling is sent to the annealing furnace for finished product annealing, and the mechanical properties of the copper-aluminum-copper composite plate are adjusted. The temperature of the annealing furnace is set to 250°C and the annealing time is 10 minutes.
[0047] The reduction ratio of the comparative example is mostly about 15%, and the reduction ratio of some deformations is lower than 15%. It is measured that the interface bonding force is deteriorated.
[0048] Comparative Example 2
[0049] The difference between this embodiment and embodiment 1 is that after rough rolling and annealing, the number of finishing rolling is changed to 8 times to obtain a 0.16 mm copper-aluminum-copper composite plate.
[0050] The specific preparation method of the copper-aluminum-copper composite plate of this comparative example is as follows:
[0051] The thickness of the copper-aluminum-copper composite plate should be about 1.11 mm after composite rolling using the rough rolling method of Example 1. The composite copper-aluminum-copper composite plate needs to be subjected to diffusion annealing treatment at an annealing temperature of 460° C. for 30 minutes to eliminate the internal stress of the copper-aluminum-copper composite plate and restore the composite plate to an O state. After diffusion annealing, the plate is cleaned to remove oil stains.
[0052] This comparative example performs 8 passes of precision rolling on the copper-aluminum-copper composite plate that has completed preliminary rolling. The thickness deformation amount each time is: 1.11mm (deformation 0.19) → 0.73mm (deformation 0.16) → 0.57mm (deformation 0.12) → 0.45mm (deformation 0.09) → 0.36mm (deformation 0.06) → 0.30mm (deformation 0.05) → 0.25mm (deformation 0.05) → 0.20mm (deformation 0.04) → 0.16mm. The finished product obtained after multiple passes of rolling is sent to the annealing furnace for finished product annealing to adjust the mechanical properties of the copper-aluminum-copper composite plate. The temperature of the annealing furnace is set to 250°C and the annealing time is 10 minutes.
[0053] The reduction ratio of this comparative example is mostly around 15%, and some exceed 21%, and the measured interface bonding strength is deteriorated.
[0054] Comparative Example 3
[0055] The difference between this comparative example and Example 1 is that after rough rolling and annealing, the number of finishing rolling is changed to 7 times to obtain a 0.16 mm copper-aluminum-copper composite plate.
[0056] The specific preparation method of the copper-aluminum-copper composite plate of this comparative example is as follows:
[0057] The thickness of the copper-aluminum-copper composite plate should be about 1.11 mm after composite rolling using the rough rolling method of Example 1. The composite copper-aluminum-copper composite plate needs to be subjected to diffusion annealing treatment at an annealing temperature of 460° C. for 30 minutes to eliminate the internal stress of the copper-aluminum-copper composite plate and restore the composite plate to an O state. After diffusion annealing, the plate is cleaned to remove oil stains.
[0058] This comparative example performs 7 passes of precision rolling on the copper-aluminum-copper composite plate that has completed preliminary rolling. The thickness deformation each time is: 1.11mm (deformation 0.20) → 0.91mm (deformation 0.18) → 0.73mm (deformation 0.17) → 0.56mm (deformation 0.14) → 0.42mm (deformation 0.13) → 0.29mm (deformation 0.08) → 0.21mm (deformation 0.05) → 0.16mm. The finished product obtained after multiple passes of rolling is sent to the annealing furnace for finished product annealing to adjust the mechanical properties of the copper-aluminum-copper composite plate. The temperature of the annealing furnace is set to 250°C and the annealing time is 10 minutes.
[0059] The reduction ratio of this comparative example is too large, the number of finishing rolling times is not enough, and the measured interface bonding strength is poor.
[0060] Comparative Example 4
[0061] The difference between this embodiment and embodiment 1 is that after rough rolling and annealing, the number of finishing rolling is changed to 6 times to obtain a 0.16 mm copper-aluminum-copper composite plate.
[0062] The specific preparation method of the copper-aluminum-copper composite plate of this comparative example is as follows:
[0063] The thickness of the copper-aluminum-copper composite plate should be about 1.11 mm after composite rolling using the rough rolling method of Example 1. The composite copper-aluminum-copper composite plate needs to be subjected to diffusion annealing treatment at an annealing temperature of 460° C. for 30 minutes to eliminate the internal stress of the copper-aluminum-copper composite plate and restore the composite plate to an O state. After diffusion annealing, the plate is cleaned to remove oil stains.
[0064] This comparative example performs 6 passes of precision rolling on the copper-aluminum-copper composite plate that has completed preliminary rolling. The thickness deformation each time is: 1.11mm (deformation 0.16) → 0.95mm (deformation 0.16) → 0.79mm (deformation 0.17) → 0.62mm (deformation 0.15) → 0.47mm (deformation 0.17) → 0.30mm (deformation 0.14) → 0.16mm. The finished product obtained after multiple passes of rolling is sent to the annealing furnace for finished product annealing to adjust the mechanical properties of the copper-aluminum-copper composite plate. The temperature of the annealing furnace is set to 250°C and the annealing time is 10 minutes.
[0065] The reduction ratio of this comparative example is too large, the number of finishing rolling times is not enough, and the measured interface bonding strength is poor.
[0066] Performance Testing
[0067] 1. Interface bonding strength test: The copper-aluminum-copper composite plates prepared in Example 1 and Comparative Examples 1-4 were used as samples, respectively, and the samples were cut into 0.16 mm × 2 mm × 2 mm blocks. The bonding strength of the samples was measured using a WDW-5 tensile testing machine. Each sample was tested 5 times, and the experimental results were averaged.
[0068] 2. Bending test: Use a bending machine to bend the sample repeatedly until it breaks and observe whether the cross section is delaminated. The above test results are shown in Table 2.
[0069] Table 2 Performance test results
[0070]
[0071] As can be seen from Table 2, the copper-aluminum-copper composite plate of the present invention has certain requirements for the single pressing amount of fine rolling during the preparation process. As can be seen from Comparative Example 1, too many fine rolling times not only reduce production efficiency, but also the pressing amount of a single rolling is not enough, which has a negative impact on the bonding strength of the metal composite, and the interface bonding strength of the final composite plate is insufficient; and as can be seen from Comparative Examples 2-4, too few fine rolling times and too much single pressing amount lead to insufficient tissue interaction at the interface composite layer, which greatly affects the interface bonding strength of the composite plate. Therefore, controlling the pressing amount of a single pass of fine rolling is the key to ensuring that the copper-aluminum-copper composite plate obtains a sufficient number of fine rolling times during the preparation process, and ensuring that the shear strength of the copper-aluminum-copper composite plate reaches more than 300MPa, and the obtained copper-aluminum-copper composite plate is repeatedly bent until it breaks, and the metal layer separation phenomenon does not occur in each layer.
[0072] The above embodiments and comparative examples demonstrate the influence of annealing temperature and the pressing amount of single-pass finishing rolling on the mechanical properties and interface bonding properties of the copper-aluminum-copper composite plate. Therefore, the present invention can provide a reference for the manufacture of ultra-thin (e.g., less than 0.2 mm) multi-layer metal composite plates that meet certain mechanical properties and interface bonding capacity requirements.
[0073] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and improvements and modifications made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the scope of protection of the present invention.
Claims
1. A high yield and high elongation copper-aluminum-copper composite plate, characterized in that: It includes upper and lower copper layers, and an intermediate aluminum layer; The copper-aluminum-copper composite plate includes a single-pass rough rolling and multiple-pass finish rolling during the rolling process; The rough rolling parameters are as follows: single-pass large-reduction rough rolling at room temperature, with a reduction rate of 70% and a rough rolling speed of 1m / min-2m / min; the copper-aluminum-copper composite plate after rough rolling is subjected to diffusion annealing treatment, with an annealing temperature of 400°C-500°C and an annealing time of 10min-60min to eliminate the internal stress of copper and restore the composite plate to an O state; The rolling parameters of the finishing rolling are as follows: the reduction rate of a single pass is 15% to 21%; the copper-aluminum-copper composite plate after finishing rolling is then heat treated, heated to 250° C.-300° C., and kept warm for 5 min-30 min.
2. The high yield and high elongation copper-aluminum-copper composite plate according to claim 1, characterized in that: The copper layer is a pure copper layer, and the thickness of the upper and lower copper layers is equal.
3. The high yield and high elongation copper-aluminum-copper composite plate according to claim 1, characterized in that: The aluminum layer is preferably an aluminum alloy, and the thickness of the aluminum layer exceeds 80%. The aluminum alloy is more preferably a 5 series aluminum alloy.
4. The high yield and high elongation copper-aluminum-copper composite plate according to claim 1, characterized in that: The aluminum alloy of the aluminum layer is selected from an aluminum alloy with a tensile strength of more than 290 MPa, a yield strength of more than 150 MPa, and an elongation of more than 24%, preferably one of 5456 aluminum alloy, 5B59 aluminum alloy, and 5056 aluminum alloy.
5. The high yield and high elongation copper-aluminum-copper composite plate according to claim 1, characterized in that: The thickness of the copper layer is 0.2mm-0.4mm, and the thickness of the aluminum alloy layer is 3.3mm-6mm; The copper-aluminum-copper composite plate is finally rolled to 0.1mm-0.2mm by rolling.
6. A method for preparing a copper-aluminum-copper composite plate with high yield and high elongation as claimed in any one of claims 1 to 5, characterized in that: The copper-aluminum-copper composite plate is obtained by rolling the copper, aluminum and copper metal plates, wherein the rolling process includes a single-pass rough rolling and multiple-pass finishing rolling; The rough rolling parameters are as follows: single-pass large-reduction rough rolling at room temperature, with a reduction rate of 70% and a rough rolling speed of 1m / min-2m / min; the copper-aluminum-copper composite plate after rough rolling is subjected to diffusion annealing treatment, with an annealing temperature of 400°C-500°C and an annealing time of 10min-60min to eliminate the internal stress of copper and restore the composite plate to an O state; The rolling parameters of the finishing rolling are as follows: the reduction rate of a single pass is 15% to 21%; the copper-aluminum-copper composite plate after finishing rolling is then heat treated, heated to 250° C.-300° C., and kept warm for 5 min-30 min.
7. The method for preparing a copper-aluminum-copper composite plate with high yield and high elongation as claimed in claim 6, characterized in that: Pre-treatment of metal sheets before rolling, including: Roughening removes the oxide film on the surface of metal sheets to expose the fresh metal inside.
8. The method for preparing a copper-aluminum-copper composite plate with high yield and high elongation as claimed in claim 7, characterized in that: After roughening, a hole is punched at the head of the metal sheet, and the three metal sheets of copper, aluminum, and copper are stacked in the order of copper, aluminum, and copper, and then the heads of the metal sheets are fixed by riveting. Furthermore, the pretreatment also includes ultrasonic cleaning of the stacked three-layer metal sheets.
9. The method for preparing a copper-aluminum-copper composite plate with high yield and high elongation as claimed in claim 7, characterized in that: The yield strength of the copper-aluminum-copper composite plate is close to 150MPa and the elongation is 14%.
10. Use of the high-yield and high-elongation copper-aluminum-copper composite plate according to any one of claims 1 to 5 in the preparation of shielding covers for 3C electronic components or Pack busbars for new energy batteries.
Citation Information
Patent Citations
Two-step composite rolling method for copper-aluminum-copper double-side ultrathin composite strip
CN102357526A
High-strength copper-aluminum-copper composite plate and preparation process thereof
CN109435371A
Preparation method for rolling multi-layer layered copper-aluminum composite ultra-thin strip at room temperature
CN113290049A
Ultra-thin aluminum-copper composite strip with ultra-thin interface and preparation method of ultra-thin aluminum-copper composite strip
CN116039175A
Clad 2xxx-series aerospace product
EP3904073A1