Production method of high-strength corrosion-resistant ship impeller forge piece
Through the forging and heat treatment of high-strength corrosion-resistant materials, combined with surface treatment and detection, the problem of insufficient structural strength and corrosion resistance of ship impeller forgings is solved, significantly improving the corrosion resistance and service life of impeller, meeting the safety of ships and Environmental protection requirements.
Patent Information
- Application Number
- CN202410961342.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
During the production and processing process, ship impeller forgings have problems such as insufficient structural strength and poor corrosion resistance, which are susceptible to seawater erosion.
Forged with high-strength corrosion-resistant materials such as stainless steel or special alloy steel. By designing forging molds and tooling, uniform heating forging is carried out, combined with heat treatment and mechanical processing, and finally special surface treatment and rigorous testing and testing are carried out to ensure the high strength of the impeller. and corrosion resistance.
It significantly improves the corrosion resistance and service life of the impeller, reduces maintenance frequency and cost, improves the safe operation level and environmental protection performance of the ship, and extends the service life of the impeller.
Smart Images

Figure CN118905119A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ship impeller forging processing, in particular to a production method of high-strength and corrosion-resistant ship impeller forgings. Background Art
[0002] Ship impeller forgings are very important components of ship power systems and are usually used in pumps, compressors, turbochargers and other equipment. Its main function is to convert energy through the action on the fluid to drive or assist the operation of the ship. Ship impeller forgings are three-dimensional, usually rotationally symmetrical mechanical components, which consist of a central hub and several blades extending outward from the hub. The impeller rotates under the action of fluids (such as water, oil, air, etc.) to achieve energy conversion. Impeller forgings are usually made of high-strength, corrosion-resistant alloy steel or stainless steel, which can withstand corrosion, wear and mechanical stress encountered in the marine environment. For example, austenitic stainless steel, martensitic stainless steel and high-temperature alloys. During the production process, ship impeller forgings need to undergo strict inspection and quality control, including dimensional inspection, non-destructive testing, material performance testing, etc., to ensure their safety and reliability in use.
[0003] At present, in the process of producing and manufacturing ship impeller forgings, the processed impeller forgings do not have good structural strength, and their corrosion resistance is poor and they are easily corroded by seawater. Therefore, it is necessary to develop a production method for high-strength and corrosion-resistant ship impeller forgings. Summary of the invention
[0004] The purpose of the present invention is to provide a method for producing high-strength and corrosion-resistant ship impeller forgings, so as to solve the problem raised in the above background technology that in the current production and manufacturing process of ship impeller forgings, the processed impeller forgings do not have good structural strength, and at the same time their corrosion resistance is poor and they are easily corroded by seawater.
[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: A method for producing high-strength, corrosion-resistant ship impeller forgings, comprising the following production method steps: S1. Select high-strength, corrosion-resistant materials suitable for the use environment of ship impellers, including stainless steel or special alloy steel, and cut the materials into required sizes to prepare blanks for forging; S2. Design and manufacture corresponding forging dies and tooling according to the working conditions and performance requirements of the impeller, and calculate and cut the required raw materials according to the size and shape of the impeller; S3. Heat the cut raw materials to the forging temperature, and keep the heating uniform to prevent stress and cracks caused by excessive temperature difference between the inside and outside of the material; S4. Forge at a controlled forging temperature, using a suitable forging ratio and deformation rate. degree, through forging, to achieve the predetermined shape and size; S5. The forged impeller needs to be heat treated, including normalizing, quenching and tempering, to optimize its mechanical properties; S6. The forged and heat-treated impeller is machined to achieve higher dimensional accuracy and surface quality; S7. The impeller surface is specially treated, including plating, anodizing and spraying; S8. The impeller is subjected to dimensional inspection, ultrasonic nondestructive testing, mechanical property testing and corrosion testing; S9. The qualified high-strength corrosion-resistant impeller is packaged to ensure that it is not damaged during transportation.
[0006] Preferably, in step S2, necessary surface treatment is performed on the raw materials, including removing the oxide layer and oil stains on the surface of the raw materials.
[0007] Preferably, the heating temperature in step S3 is higher than the recrystallization temperature of the metal to facilitate hot forging.
[0008] Preferably, in step S4, pressure is applied to the forging blank at high temperature to cause it to undergo plastic deformation to form a preliminary shape of the impeller, and the forging forms include free forging and die forging, wherein the die forging can be open or closed.
[0009] Preferably, in step S5, the heating temperature is controlled at 910° C. and maintained for a period of time, followed by oil quenching, and then heated to 520° C. for tempering.
[0010] Preferably, the tempering time in S5 is controlled to be 1 hour.
[0011] Compared with the prior art, the present invention has the following beneficial effects: (1) The high-strength corrosion-resistant material produced by the production method of the invention can resist corrosion in the marine environment, thereby significantly improving the service life of the impeller and ensuring the reliability and stability of the impeller under complex conditions. Due to the improved corrosion resistance, the maintenance frequency and cost of the impeller are greatly reduced; (2) Through precision forging technology, the impeller can be made lightweight, which can reduce the burden on the ship and reduce energy consumption. Good mechanical properties and corrosion resistance reduce failures caused by material fatigue or corrosion and improve the safe operation level of the ship. The impeller made by the above method helps the ship meet emission and environmental protection requirements. The service life of the impeller is extended, the replacement frequency is reduced, and long-term economic benefits are brought to the shipowner. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a flowchart of the steps of the production method of the present invention. DETAILED DESCRIPTION
[0013] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0014] See also Figure 1 An embodiment of the present invention is as follows: a method for producing high-strength and corrosion-resistant ship impeller forgings, comprising the following production method steps: S1. Select high-strength and corrosion-resistant materials suitable for the use environment of ship impellers, including stainless steel or special alloy steel, and cut the materials into required sizes to prepare blanks for forging; S2. Design and manufacture corresponding forging dies and tooling according to the working conditions and performance requirements of the impeller, and calculate and cut the required raw materials according to the size and shape of the impeller; S3. Heat the cut raw materials to the forging temperature, and keep the heating uniform to prevent the temperature difference between the inside and outside of the material from being too large to generate stress and cracks; S4. Forge at a controlled forging temperature, using a suitable forging ratio and deformation rate. degree, through forging, to achieve the predetermined shape and size; S5. The forged impeller needs to be heat treated, including normalizing, quenching and tempering, to optimize its mechanical properties; S6. The forged and heat-treated impeller is machined to achieve higher dimensional accuracy and surface quality; S7. The impeller surface is specially treated, including plating, anodizing and spraying; S8. The impeller is subjected to dimensional inspection, ultrasonic nondestructive testing, mechanical property testing and corrosion testing; S9. The qualified high-strength corrosion-resistant impeller is packaged to ensure that it is not damaged during transportation.
[0015] Furthermore, in step S2, necessary surface treatment is performed on the raw materials, including removing the oxide layer and oil stains on the surface of the raw materials.
[0016] Furthermore, the heating temperature in step S3 should be higher than the recrystallization temperature of the metal to facilitate hot forging.
[0017] Furthermore, in step S4, pressure is applied to the forging blank at high temperature to cause it to undergo plastic deformation to form a preliminary shape of the impeller. The forging forms include free forging and die forging, wherein the die forging can be open or closed.
[0018] Furthermore, in step S5, the heating temperature is controlled at 910° C. and maintained for a period of time, followed by oil quenching, and then heated to 520° C. for tempering.
[0019] Furthermore, the tempering time in S5 is controlled to be 1 hour. Example
[0020] Heat the cut raw materials to the forging temperature. Keep the heating uniform to prevent the temperature difference between the inside and outside of the material from being too large to cause stress and cracks. Forge at a controlled forging temperature, use a suitable forging ratio and deformation speed, and forge to achieve the predetermined shape and size. The forged impeller needs to be heat treated, including normalizing, quenching and tempering. Keep the heating temperature at 910℃ for a period of time, then oil quench, and then heat to 520℃ for tempering. The tempering time in S5 is controlled at 1 hour.
[0021] Comparative Example 1 Heat the cut raw materials to the forging temperature. Keep the heating uniform to prevent the temperature difference between the inside and outside of the material from being too large to cause stress and cracks. Forge at a controlled forging temperature, use a suitable forging ratio and deformation speed, and forge to achieve the predetermined shape and size. The forged impeller needs to be heat treated, including normalizing, quenching and tempering. Control the heating temperature at 950℃ for a period of time, then oil quench, and then heat to 520℃ for tempering. The tempering time in S5 is controlled at 1 hour.
[0022] Comparative Example 2 Heat the cut raw materials to the forging temperature. Keep the heating uniform to prevent the temperature difference between the inside and outside of the material from being too large to cause stress and cracks. Forge at a controlled forging temperature, use a suitable forging ratio and deformation speed, and forge to achieve the predetermined shape and size. The forged impeller needs to be heat treated, including normalizing, quenching and tempering. Keep the heating temperature at 1000℃ for a period of time, then oil quench, and then heat to 520℃ for tempering. The tempering time in S5 is controlled at 1 hour.
[0023] Through the test of Example 1 and Comparative Examples 1 and 2, it was found that with the gradual increase of the heating temperature, the structural strength and corrosion resistance of the obtained impeller material were significantly improved.
[0024] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
Claims
1. A method for producing high-strength, corrosion-resistant ship impeller forgings. It is characterized in that The method comprises the following steps: S1. Select high-strength and corrosion-resistant materials suitable for the use environment of ship impellers, including stainless steel or special alloy steel, and cut the materials into required sizes to prepare billets for forging; S2. Design and manufacture corresponding forging dies and tooling according to the working conditions and performance requirements of the impeller, and calculate and cut the required raw materials according to the size and shape of the impeller; S3. Heat the cut raw materials to the forging temperature. Keep the heating uniform to prevent the temperature difference between the inside and outside of the material from causing stress and cracks. S4. Forging is performed at a controlled forging temperature, using a suitable forging ratio and deformation speed, and achieving a predetermined shape and size through forging; S5. After forging, the impeller needs to be heat treated, including normalizing, quenching and tempering, to optimize its mechanical properties; S6. Machining the forged and heat-treated impeller to achieve higher dimensional accuracy and surface quality; S7. Special treatment of the impeller surface, including plating, anodizing and spraying; S8. Perform dimensional inspection, ultrasonic nondestructive testing, mechanical property testing and corrosion testing on the impeller; S9. Pack the high-strength corrosion-resistant impellers that have passed the inspection to ensure that they are not damaged during transportation.
2. The method for producing a high-strength, corrosion-resistant ship impeller forging according to claim 1, Features: In step S2, necessary surface treatment is performed on the raw materials, including removing the oxide layer and oil stains on the surface of the raw materials.
3. The method for producing a high-strength, corrosion-resistant ship impeller forging according to claim 1, Features: The heating temperature in step S3 should be higher than the recrystallization temperature of the metal to facilitate hot forging.
4. The method for producing a high-strength, corrosion-resistant ship impeller forging according to claim 1, Features: In the step S4, pressure is applied to the forging blank at high temperature to cause it to undergo plastic deformation and form a preliminary shape of the impeller. The forging forms include free forging and die forging, wherein the die forging can be open or closed.
5. The method for producing a high-strength, corrosion-resistant ship impeller forging according to claim 1, Features: In step S5, the heating temperature is controlled at 910° C. and maintained for a period of time, followed by oil quenching, and then heated to 520° C. for tempering.
6. The method for producing a high-strength, corrosion-resistant ship impeller forging according to claim 1, Features: The tempering time in S5 is controlled to be 1 hour.