Anti-corrosion and anti-fouling coating material as well as preparation method and application thereof

Through the synergistic action of nano-silicon dioxide, epoxy resin and other materials, a dense protective film is formed, which solves the problems of poor adhesion and insufficient corrosion resistance of marine anti-corrosion coatings, and achieves efficient anti-corrosion and pollution-proofing effects on marine engineering facilities.

CN118909517AInactive Publication Date: 2024-11-08SICHUAN TONGSHEN WATERPROOF ENG CO LTD

Patent Information

Application Number
CN202411110058.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing marine anticorrosion coatings have insufficient performance in seawater erosion and marine biological pollution, and have poor adhesion, resulting in accelerated corrosion of metal facilities and shortened service life.

Method used

Anti-corrosion and anti-fouling coating materials using nano-silica, bisphenol A type epoxy resin, silicone resin, cerium salt, algae, phosphate, fungicide and other raw materials, and the adhesion of the coating is improved through synergistic effects. Anti-corrosion and anti-fouling properties form a dense protective film.

Benefits of technology

It significantly improves the corrosion resistance, wear resistance and durability of the coating, extends the service life, prevents marine biological adhesion and chemical corrosion, and enhances the protection effect of marine engineering facilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991911570000121
    Figure BDA0004991911570000121
Patent Text Reader

Abstract

The invention relates to the field of marine anti-corrosion and anti-fouling coating materials, and discloses an anti-corrosion and anti-fouling coating material as well as a preparation method and application thereof. The coating comprises the following raw materials in parts by mass: 3-4 parts of nano silicon dioxide, 20-30 parts of epoxy resin, 20-30 parts of a curing agent, 10-25 parts of organic silicon resin, 4-6 parts of cerium salt, 12-14 parts of seaweed gel, 6-12 parts of phosphate, 1-3 parts of a dispersant, 1-3 parts of a stabilizer, 5-10 parts of a bactericide, 1-3 parts of an auxiliary agent and 60-100 parts of a solvent. The epoxy resin is bisphenol A epoxy resin; the curing agent is an amino silane curing agent. According to the anti-corrosion and anti-fouling coating material provided by the invention, the compatibility among the raw materials is good. Through the synergistic effect of various raw materials, the adhesion of the coating on a base material and excellent corrosion resistance and antifouling performance are guaranteed, and long-acting protection on ocean engineering facilities can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of marine anti-corrosion and anti-fouling coating materials, and in particular to an anti-corrosion and anti-fouling coating material and a preparation method and application thereof. Background Art

[0002] With the rapid development of my country's marine economy, the corrosion protection of ships and marine engineering facilities has become an important issue that needs to be solved urgently. At present, most marine engineering facilities use metal shells, including steel, titanium alloy and aluminum alloy. These metal shells are in the marine environment for a long time, and will be affected by seawater temperature, seawater salinity, marine atmospheric temperature, marine atmospheric humidity and the attachment of marine organisms, and will suffer from varying degrees of corrosion. Therefore, the marine environment is an extremely harsh corrosive environment. The seawater and marine atmosphere have a high salt content, including high concentrations of Cl - Mg 2+ and SO4 2- etc.; and the corrosion environment is affected by conditions such as sunshine, sea breeze, and marine life; marine biofouling is the result of marine life attaching to and growing on the substrate surface, which will produce a series of serious consequences, not only increasing the consumption and maintenance times of marine equipment such as ships, but also destroying the coating on the metal surface, thereby accelerating metal corrosion and aging, and further affecting the performance of marine functional facilities. Therefore, seawater, marine atmosphere, and marine life are the main causes of corrosion and pollution of marine engineering facilities. When the facilities are corroded, it will lead to equipment downtime, material failure, and other problems, wasting precious resources and seriously affecting the service safety and service life of marine engineering facilities.

[0003] In order to protect metals from seawater corrosion and damage from marine organisms in the marine environment, the current conventional technology is to apply a protective coating on the surface of marine engineering facilities, and the development prospects of marine anti-corrosion coatings are becoming more and more promising. The special environment of the ocean requires that marine anti-corrosion coatings must have high corrosion resistance, scratch resistance and weather resistance. The overall performance of current marine anti-corrosion coatings is relatively weak. After being eroded by seawater for a long time, they may lose their original anti-corrosion effect and are easily polluted by marine organisms. The attachment and growth of a large number of algae and harmful substances destroy the coating surface and accelerate the corrosion of the metal surface by seawater. In addition, some marine anti-corrosion coatings have poor adhesion, resulting in pores and bubbles on the paint surface, causing irreversible damage to the paint surface. Therefore, there is an urgent need for a high-performance and high-quality marine anti-corrosion and anti-fouling material to increase the service life of marine engineering facilities. Summary of the invention

[0004] In view of this, the present invention proposes an anti-corrosion and anti-fouling coating material and a preparation method and application thereof to solve the problems in the prior art that seawater anti-corrosion coatings have poor adhesion effect, short anti-corrosion time and cannot effectively prevent the attachment of marine organisms.

[0005] The present invention provides an anti-corrosion and anti-fouling coating material, comprising the following raw materials in parts by weight:

[0006] 3-4 parts of nano silicon dioxide, 20-30 parts of epoxy resin, 20-30 parts of curing agent, 10-25 parts of silicone resin, 4-6 parts of cerium salt, 12-14 parts of alginate, 6-12 parts of phosphate, 1-3 parts of dispersant, 1-3 parts of stabilizer, 5-10 parts of bactericide, 1-3 parts of auxiliary agent, 60-100 parts of solvent;

[0007] The epoxy resin is bisphenol A epoxy resin;

[0008] The curing agent is an aminosilane curing agent.

[0009] Furthermore, the particle size of the nano-silicon dioxide is 3-5 nanometers.

[0010] Furthermore, the organic silicone resin is polydimethylsiloxane.

[0011] Further, the cerium salt is selected from one or more of cerous oxalate, cerous sulfate, cerous chloride and cerous nitrate;

[0012] The phosphate is selected from one or more of orthophosphate, polyphosphate and phosphite;

[0013] The dispersant is selected from one or more of BYK-110, BYK-161, BYK-163 and BYK-ATU.

[0014] Further, the stabilizer is selected from quaternary ammonium salt stabilizers or quaternary ammonium base stabilizers;

[0015] The bactericide is selected from cuprous oxide, thiophanate-methyl and diuron;

[0016] The mass ratio of cuprous oxide, thiophanate-methyl and diuron is 2-7:1:1.

[0017] Further, the auxiliary agent includes one or more of a wetting agent, a leveling agent and a defoaming agent;

[0018] The wetting agent is BYK-538N wetting agent, the leveling agent is selected from one or more of polyether-modified polydimethylsiloxane, acrylate copolymer and fluorocarbon polymer, and the defoamer is BYK-141 defoamer;

[0019] The solvent is a mixed solvent of xylene / n-butanol.

[0020] The present invention also provides a method for preparing the anti-corrosion and anti-fouling coating material, comprising the following preparation steps:

[0021] (1) mixing epoxy resin, curing agent, silicone resin and solvent in proportion to obtain material A;

[0022] (2) adding nano-silicon dioxide, cerium salt and phosphate to material A, stirring and standing to obtain material B;

[0023] (3) Adding alginate, a dispersant, a stabilizer, a bactericide and an auxiliary agent to material B to obtain material C, grinding and sieving material C to obtain the anti-corrosion and anti-fouling coating material.

[0024] Furthermore, the stirring rate of the mixing in step (1) is 500-800 rpm, and the mixing time is 8-12 min;

[0025] In step (2), the stirring rate is 2000-3000 rpm, the stirring time is 4-8 hours, and the standing time is 20-50 minutes.

[0026] Furthermore, the stirring rate of the mixing in step (3) is 1500-2500 rpm, and the stirring time is 2-6 h;

[0027] The mesh number of the sieving is 120-140 meshes.

[0028] The present invention also provides application of the anti-corrosion and anti-fouling coating material in marine anti-corrosion coating.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention provides an anti-corrosion and anti-fouling coating material, comprising the following raw materials in parts by weight:

[0031] 3-4 parts of nano silicon dioxide, 20-30 parts of epoxy resin, 20-30 parts of curing agent, 10-25 parts of silicone resin, 4-6 parts of cerium salt, 12-14 parts of alginate, 6-12 parts of phosphate, 1-3 parts of dispersant, 1-3 parts of stabilizer, 5-10 parts of bactericide, 1-3 parts of auxiliary agent, 60-100 parts of solvent. In the anti-corrosion and anti-fouling coating material provided by the present invention, the compatibility between the raw materials is good. Through the synergistic effect between the various raw materials, the adhesion of the coating on the substrate and the excellent anti-corrosion and anti-fouling performance are guaranteed, and long-term protection of marine engineering facilities can be achieved.

[0032] Nano-silicon dioxide is small in size and can fill the pores of the coating. At the same time, it has a large specific surface area and can form cross-links with polymers to make the coating denser. It effectively blocks the penetration of corrosive media such as moisture and oxygen, thereby improving the corrosion resistance of the coating. Nano-silicon dioxide also has good adsorption properties and can adsorb harmful substances on the surface of the coating, such as oil, dust, etc., thereby improving the anti-fouling properties of the coating. In addition, nano-silicon dioxide can enhance the hardness and wear resistance of the coating, improve the durability and heat resistance of the coating, and extend the service life of the coating.

[0033] The epoxy resin selected by the present invention is bisphenol A type epoxy resin, which has extremely strong adhesion to metal. This characteristic enables the coating to be firmly attached to the substrate surface, forming a dense protective film, and cooperating with nano silicon dioxide, further isolating the direct contact of corrosive media (such as water, oxygen, chemicals, etc.) with the substrate, thereby extending the service life of the coating and protecting the substrate. And the anti-corrosion and anti-fouling coating is not easy to crack or fall off when subjected to external force impact or temperature change, thereby maintaining the integrity and protective effect of the coating. Bisphenol A type epoxy resin has excellent chemical corrosion resistance after curing, and can resist the erosion of various chemical substances such as acid, alkali, salt, etc. The epoxy resin also possesses high electrical insulation, which is conducive to preventing electrochemical corrosion and ensuring the safe operation of electrical equipment.

[0034] The organic silicone resin selected by the present invention is polydimethylsiloxane, which has a lower surface tension, can reduce the viscosity of the coating, improve its fluidity and smoothness of coating. This makes it easier for the coating to be evenly distributed on the substrate, reduces the generation of bubbles and defects, and improves the overall quality of the coating. Durability: polydimethylsiloxane can form a flexible protective layer after the coating dries, and this protective layer can significantly enhance the wear resistance, scratch resistance, chemical corrosion resistance and pollution resistance of the coating, thereby extending the service life of the coating. Working together with nano-silicon dioxide, both have extremely low surface energy, making it difficult for fouling organisms and pollutants to adhere to the surface of the coating or adhere loosely, thereby achieving the purpose of anti-fouling. Polydimethylsiloxane can also effectively resist moisture penetration and moisture absorption of the coating, improving the moisture resistance and durability of the coating. In a high temperature environment, it can maintain the stability of the coating to prevent deformation and peeling; in a low temperature environment, it can maintain the softness and elasticity of the coating to prevent cracking and falling off.

[0035] As an effective corrosion inhibitor, cerium salt can significantly inhibit the corrosion process on the metal surface. It forms a dense protective film by adsorbing on the metal surface, blocking the direct contact between the corrosive medium (such as oxygen, water, ammonia ions, etc.) and the metal substrate, thereby slowing down or preventing the occurrence of corrosion. When used in combination with bisphenol A epoxy resin, cerium salt can form a composite coating with higher corrosion resistance. This composite coating not only combines the corrosion inhibition performance of cerium salt and the excellent film-forming performance of bisphenol A epoxy resin, but also further enhances the anti-corrosion effect of the coating through the interaction between the two. The addition of cerium salt can also improve the physical properties of the coating, and improve the hardness, wear resistance, impact resistance, etc. of the coating. The improvement of these properties helps the coating maintain integrity and stability in harsh environments, thereby better playing an anti-corrosion and anti-fouling role.

[0036] Phosphates have excellent chemical stability and can resist corrosion from a variety of chemicals, protecting the substrate from corrosion.

[0037] The bactericides in the present invention are cuprous oxide, thiophanate-methyl and diuron. Cuprous oxide is a low-toxic antibacterial agent that can release copper ions to kill harmful substances and improve the hardness and wear resistance of the coating. Chlorothalonil and diuron can effectively kill algae species. After the three components are compounded, they have a special bactericidal effect on algae and are low in toxicity, effectively improving the attachment and growth of algae and harmful substances on the surface of marine engineering facilities. DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] The present invention provides an anti-corrosion and anti-fouling coating material, comprising the following raw materials in parts by weight:

[0040] 3-4 parts of nano silicon dioxide, 20-30 parts of epoxy resin, 20-30 parts of curing agent, 10-25 parts of silicone resin, 4-6 parts of cerium salt, 12-14 parts of alginate, 6-12 parts of phosphate, 1-3 parts of dispersant, 1-3 parts of stabilizer, 5-10 parts of bactericide, 1-3 parts of auxiliary agent, 60-100 parts of solvent;

[0041] The epoxy resin is bisphenol A epoxy resin;

[0042] The curing agent is an aminosilane curing agent.

[0043] In one embodiment, the mass fraction of the nano-silicon dioxide is preferably 3.2-3.8 parts, more preferably 3.3-3.7 parts, and more preferably 3.4-3.6 parts.

[0044] In one embodiment, the weight fraction of the epoxy resin is preferably 22-28 parts, more preferably 23-27 parts, and more preferably 24-26 parts.

[0045] In one embodiment, the mass fraction of the curing agent is preferably 22-28 parts, more preferably 23-27 parts, and more preferably 24-26 parts.

[0046] In one embodiment, the weight fraction of the silicone resin is preferably 12-23 parts, more preferably 14-21 parts, and more preferably 16-19 parts.

[0047] In one embodiment, the mass fraction of the cerium salt is preferably 4.2-5.8 parts, more preferably 4.5-5.5 parts, and more preferably 4.8-5.2 parts.

[0048] In one embodiment, the mass fraction of the alginate is preferably 12.2-13.8 parts, more preferably 12.5-13.5 parts, and more preferably 12.7-13.3 parts.

[0049] In one embodiment, the mass fraction of the phosphate is preferably 7-11 parts, more preferably 8-10 parts, and more preferably 8.5-9.5 parts.

[0050] In one embodiment, the mass fraction of the dispersant is preferably 1.2-2.8 parts, more preferably 1.5-2.5 parts, and more preferably 1.8-2.2 parts.

[0051] In one embodiment, the weight fraction of the stabilizer is preferably 1.2-2.8 parts, more preferably 1.5-2.5 parts, and more preferably 1.9-2.1 parts.

[0052] In one embodiment, the mass fraction of the fungicide is preferably 6-9 parts, more preferably 6.5-8.5 parts, and more preferably 7-8 parts.

[0053] In one embodiment, the weight fraction of the auxiliary agent is preferably 1.3-2.7 parts, more preferably 1.7-2.3 parts, and more preferably 1.8-2.1 parts.

[0054] In one embodiment, the mass fraction of the solvent is preferably 70-90 parts, more preferably 75-85 parts, and more preferably 78-83 parts.

[0055] In one embodiment, the particle size of the nano-silicon dioxide is preferably 3-5 nanometers, more preferably 3.5-4.5 nanometers, and more preferably 4 nanometers.

[0056] In one embodiment, the silicone resin is preferably polydimethylsiloxane.

[0057] In one embodiment, the cerium salt is preferably selected from one or more of cerous oxalate, cerous sulfate, cerous chloride and cerous nitrate;

[0058] The phosphate is preferably selected from one or more of orthophosphate, polyphosphate and phosphite;

[0059] The dispersant is preferably selected from one or more of BYK-110, BYK-161, BYK-163 and BYK-ATU.

[0060] In one embodiment, the stabilizer is preferably selected from quaternary ammonium salt stabilizers or quaternary ammonium base stabilizers;

[0061] The bactericide is preferably selected from cuprous oxide, thiophanate-methyl and diuron;

[0062] The mass ratio of cuprous oxide, thiophanate-methyl and diuron is preferably 2-7:1:1, more preferably 3-6:1:1, and more preferably 4-5:1:1.

[0063] In one embodiment, the auxiliary agent preferably includes one or more of a wetting agent, a leveling agent and a defoaming agent;

[0064] The wetting agent is preferably BYK-538N wetting agent, the leveling agent is preferably selected from one or more of polyether-modified polydimethylsiloxane, acrylate copolymer and fluorocarbon polymer, and the defoamer is preferably BYK-141 defoamer;

[0065] The solvent is preferably a mixed solvent of xylene / n-butanol.

[0066] The present invention also provides a method for preparing the anti-corrosion and anti-fouling coating material, comprising the following preparation steps:

[0067] (1) mixing epoxy resin, curing agent, silicone resin and solvent in proportion to obtain material A;

[0068] (2) adding nano-silicon dioxide, cerium salt and phosphate to material A, stirring and standing to obtain material B;

[0069] (3) Adding alginate, a dispersant, a stabilizer, a bactericide and an auxiliary agent to material B to obtain material C, grinding and sieving material C to obtain the anti-corrosion and anti-fouling coating material.

[0070] In one embodiment, the stirring rate of the mixing in step (1) is preferably 500-800 rpm, more preferably 600-700 rpm, more preferably 640-660 rpm, and the mixing time is preferably 8-12 min, more preferably 8.5-11.5 min, more preferably 9-11 min;

[0071] The stirring rate in step (2) is preferably 2000-3000 rpm, more preferably 2200-2800 rpm, more preferably 2400-2600 rpm, the stirring time is preferably 4-8 h, more preferably 5-7 h, more preferably 6 h, and the standing time is preferably 20-50 min, more preferably 30-40 min, more preferably 34-36 min.

[0072] In one embodiment, the stirring rate of the mixing in step (3) is preferably 1500-2500 rpm, more preferably 1700-2300 rpm, more preferably 1900-2100 rpm, and the stirring time is preferably 2-6 h, more preferably 3-5 h, more preferably 4 h;

[0073] The mesh size of the sieve is preferably 120-140 mesh, and more preferably 130 mesh.

[0074] The present invention also provides application of the anti-corrosion and anti-fouling coating material in marine anti-corrosion coating.

[0075] Example 1

[0076] The particle size of nano-silica is 3 nanometers, the epoxy resin is bisphenol A epoxy resin, the curing agent is aminosilane curing agent, the silicone resin is polydimethylsiloxane, the cerium salt is cerium oxalate, the phosphate is orthophosphate, the dispersant is BYK-110, the stabilizer is a quaternary ammonium salt stabilizer, the mass ratio of cuprous oxide, thiophanate-methyl and diuron in the fungicide is 2:1:1, and the auxiliary agent is BYK-538N wetting agent.

[0077] 3 parts of nano silicon dioxide, 20 parts of epoxy resin, 20 parts of curing agent, 10 parts of silicone resin, 4 parts of cerium salt, 12 parts of alginate, 6 parts of phosphate, 1 part of dispersant, 1 part of stabilizer, 5 parts of bactericide, 1 part of auxiliary agent, and 60 parts of solvent.

[0078] (1) mixing epoxy resin, curing agent, silicone resin and solvent in proportion at a speed of 500 rpm for 8 min to obtain material A;

[0079] (2) adding nano-silicon dioxide, cerium salt and phosphate to material A, stirring at a rate of 2000 rpm for 4 hours, and then standing for 20 minutes to obtain material B;

[0080] (3) Adding alginate, dispersant, stabilizer, bactericide and adjuvant to material B, mixing at a rate of 1500 rpm for 2 h to obtain material C, grinding material C and passing it through a 120-mesh sieve to obtain the anti-corrosion and anti-fouling coating material.

[0081] Example 2

[0082] The particle size of nano-silica is 4 nanometers, the epoxy resin is bisphenol A epoxy resin, the curing agent is aminosilane curing agent, the silicone resin is polydimethylsiloxane, the cerium salt is cerous sulfate, the phosphate is polyphosphate, the dispersant is BYK-161, the stabilizer is a quaternary ammonium salt stabilizer, the mass ratio of cuprous oxide, thiophanate-methyl and diuron in the fungicide is 7:1:1, and the additives are BYK-538N wetting agent and BYK-141 defoaming agent.

[0083] 4 parts of nano silicon dioxide, 30 parts of epoxy resin, 30 parts of curing agent, 25 parts of silicone resin, 6 parts of cerium salt, 14 parts of alginate, 12 parts of phosphate, 3 parts of dispersant, 3 parts of stabilizer, 10 parts of bactericide, 3 parts of auxiliary agent, and 100 parts of solvent.

[0084] (1) mixing epoxy resin, curing agent, silicone resin and solvent in proportion at a speed of 600 rpm for 8.5 min to obtain material A;

[0085] (2) adding nano-silicon dioxide, cerium salt and phosphate to material A, stirring at a rate of 2200 rpm for 5 h, and then standing for 30 min to obtain material B;

[0086] (3) Adding alginate, dispersant, stabilizer, bactericide and adjuvant to material B, mixing at a rate of 1700 rpm for 3 h to obtain material C, grinding material C and passing it through a 120-mesh sieve to obtain the anti-corrosion and anti-fouling coating material.

[0087] Example 3

[0088] The particle size of nano-silica is 4 nanometers, the epoxy resin is bisphenol A epoxy resin, the curing agent is aminosilane curing agent, the silicone resin is polydimethylsiloxane, the cerium salt is cerium nitrate, the phosphate is polyphosphate, the dispersant is BYK-161, the stabilizer is a quaternary ammonium salt stabilizer, the mass ratio of cuprous oxide, thiophanate-methyl and diuron in the fungicide is 3:1:1, and the additives are BYK-538N wetting agent and BYK-141 defoaming agent.

[0089] 3.2 parts of nano silicon dioxide, 22 parts of epoxy resin, 22 parts of curing agent, 12 parts of silicone resin, 4.2 parts of cerium salt, 12.2 parts of alginate, 7 parts of phosphate, 1.2 parts of dispersant, 1.2 parts of stabilizer, 6 parts of bactericide, 1.3 parts of auxiliary agent, and 70 parts of solvent.

[0090] (1) mixing epoxy resin, curing agent, silicone resin and solvent in proportion at a speed of 700 rpm for 8 min to obtain material A;

[0091] (2) adding nano-silicon dioxide, cerium salt and phosphate to material A, stirring at a rate of 2300 rpm for 4 hours, and then standing for 20 minutes to obtain material B;

[0092] (3) Adding alginate, dispersant, stabilizer, bactericide and adjuvant to material B, mixing at a rate of 1500 rpm for 3 h to obtain material C, grinding material C and passing it through a 120-mesh sieve to obtain the anti-corrosion and anti-fouling coating material.

[0093] Example 4

[0094] The particle size of nano-silica is 3 nanometers, the epoxy resin is bisphenol A epoxy resin, the curing agent is aminosilane curing agent, the silicone resin is polydimethylsiloxane, the cerium salt is cerium nitrate, the phosphate is phosphite, the dispersant is BYK-163, the stabilizer is a quaternary ammonium salt stabilizer, the mass ratio of cuprous oxide, thiophanate-methyl and diuron in the fungicide is 4:1:1, and the additives are BYK-538N wetting agent and BYK-141 defoaming agent.

[0095] 3.7 parts of nano silicon dioxide, 23 parts of epoxy resin, 23 parts of curing agent, 21 parts of silicone resin, 5.5 parts of cerium salt, 12.5 parts of alginate, 10 parts of phosphate, 2.5 parts of dispersant, 2.5 parts of stabilizer, 8.5 parts of bactericide, 1.7 parts of auxiliary agent, and 85 parts of solvent.

[0096] (1) mixing epoxy resin, curing agent, silicone resin and solvent in proportion at a speed of 660 rpm for 9 minutes to obtain material A;

[0097] (2) adding nano-silicon dioxide, cerium salt and phosphate to material A, stirring at a rate of 2400 rpm for 4 hours, and then standing for 36 minutes to obtain material B;

[0098] (3) Adding alginate, dispersant, stabilizer, bactericide and adjuvant to material B, mixing at a rate of 1900 rpm for 2 h to obtain material C, grinding material C and passing it through a 120-mesh sieve to obtain the anti-corrosion and anti-fouling coating material.

[0099] Example 5

[0100] The particle size of nano-silica is 3 nanometers, the epoxy resin is bisphenol A epoxy resin, the curing agent is aminosilane curing agent, the silicone resin is polydimethylsiloxane, the cerium salt is cerium nitrate, the phosphate is phosphite, the dispersant is BYK-163, the stabilizer is a quaternary ammonium salt stabilizer, the mass ratio of cuprous oxide, thiophanate-methyl and diuron in the fungicide is 4:1:1, and the auxiliary agent is a leveling agent of polyether modified polydimethylsiloxane.

[0101] 3.6 parts of nano silicon dioxide, 26 parts of epoxy resin, 26 parts of curing agent, 19 parts of silicone resin, 5.2 parts of cerium salt, 13.3 parts of alginate, 9.5 parts of phosphate, 2.2 parts of dispersant, 2.1 parts of stabilizer, 8 parts of bactericide, 2.1 parts of auxiliary agent and 83 parts of solvent.

[0102] (1) mixing epoxy resin, curing agent, silicone resin and solvent in proportion at a speed of 660 rpm for 11 min to obtain material A;

[0103] (2) adding nano-silicon dioxide, cerium salt and phosphate to material A, stirring at a rate of 2600 rpm for 6 hours, and then standing for 34 minutes to obtain material B;

[0104] (3) Adding alginate, a dispersant, a stabilizer, a bactericide and an auxiliary agent to material B, mixing at a rate of 2100 rpm for 4 hours to obtain material C, grinding and sieving material C to obtain the anti-corrosion and anti-fouling coating material.

[0105] Performance Testing

[0106] The anti-corrosion and anti-fouling coating materials obtained in Examples 1-5 were subjected to seawater immersion tests.

[0107] Experimental process: Select 5 identical 3-cubic-meter steel square buoys, and conduct anti-corrosion and anti-fouling tests on the outer surfaces: Derust the 5 sides of the square buoy to achieve Sa2.5 level rust removal effect, and leave one side untreated for rust-resistant anti-corrosion and anti-fouling coating test. Use a roller brush to apply the anti-corrosion and anti-fouling coating material 4 times, with an interval of 30-40 minutes between each time. After the coating is completed, cure for 48 hours, and the dry film thickness is 300±50μm. After the coating is completely dry, put it in seawater for immersion test, and observe the changes in the immersion test process every 10 days.

[0108] Experimental results: After 3 months of seawater immersion test, the coating surfaces of Examples 1-5 were smooth and flat, without rust, cracking, peeling or peeling. There was no marine organism attachment and growth on the coating surface, which fully met the requirements of ship anti-corrosion and anti-fouling.

[0109] A rusted steel plate was prepared by placing a 100×50×3 mm steel plate in a 5% NaCl salt spray box for 7 days for rust treatment, and then polishing the rust to St2 level.

[0110] The anti-corrosion and anti-fouling coating materials obtained in Examples 1-5 were applied to the above five steel plates with a roller brush to obtain different surfaces of rusted steel plates with a coating thickness of 350 μm. After the coating was cured, the edges of the steel plates were sealed and then tested for 4000 h salt spray resistance and 4000 h moisture and heat resistance. The results are shown in Table 1:

[0111] Table 1 4000h salt spray resistance and 4000h humidity and heat resistance test results of the anticorrosion and antifouling coating materials of Examples 1-5

[0112]

[0113] It should be noted that the decrease in weight loss rate (%) indicates the percentage of mass lost by the coating after 4000 hours of testing. The smaller the value, the better the coating is maintained in a corrosive environment. The decrease in adhesion (%) indicates the percentage of adhesion decrease of the coating after the test. The smaller the value, the better the bonding between the coating and the substrate. The rust condition (% area) indicates the percentage of rusted area on the coating surface obtained based on image recognition technology. The smaller the value, the better.

[0114] It can be seen from Table 1 that the anti-corrosion and anti-fouling coating material provided by the present invention has excellent weather resistance and can effectively improve the corrosion resistance of metal materials in complex environments.

[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. An anti-corrosion and anti-fouling coating material, characterized in that: Contains the following raw materials in parts by weight: 3-4 parts of nano silicon dioxide, 20-30 parts of epoxy resin, 20-30 parts of curing agent, 10-25 parts of silicone resin, 4-6 parts of cerium salt, 12-14 parts of alginate, 6-12 parts of phosphate, 1-3 parts of dispersant, 1-3 parts of stabilizer, 5-10 parts of bactericide, 1-3 parts of auxiliary agent, 60-100 parts of solvent; The epoxy resin is bisphenol A epoxy resin; The curing agent is an aminosilane curing agent.

2. The anti-corrosion and anti-fouling coating material according to claim 1, characterized in that: The particle size of the nano silicon dioxide is 3-5 nanometers.

3. An anti-corrosion and anti-fouling coating material as claimed in claim 1 or 2, characterized in that: The organic silicone resin is polydimethylsiloxane.

4. The anti-corrosion and anti-fouling coating material according to claim 3, characterized in that: The cerium salt is selected from one or more of cerous oxalate, cerous sulfate, cerous chloride and cerous nitrate; The phosphate is selected from one or more of orthophosphate, polyphosphate and phosphite; The dispersant is selected from one or more of BYK-110, BYK-161, BYK-163 and BYK-ATU.

5. The anti-corrosion and anti-fouling coating material according to claim 4, characterized in that: The stabilizer is selected from quaternary ammonium salt stabilizers or quaternary ammonium base stabilizers; The bactericide is selected from cuprous oxide, thiophanate-methyl and diuron; The mass ratio of cuprous oxide, thiophanate-methyl and diuron is 2-7:1:

1.

6. An anti-corrosion and anti-fouling coating material as claimed in claim 4 or 5, characterized in that: The auxiliary agent includes one or more of a wetting agent, a leveling agent and a defoaming agent; The wetting agent is BYK-538N wetting agent, the leveling agent is selected from one or more of polyether-modified polydimethylsiloxane, acrylate copolymer and fluorocarbon polymer, and the defoamer is BYK-141 defoamer; The solvent is a mixed solvent of xylene / n-butanol.

7. The method for preparing an anticorrosion and antifouling coating material according to any one of claims 1 to 6, characterized in that: The preparation steps include: (1) mixing epoxy resin, curing agent, silicone resin and solvent in proportion to obtain material A; (2) adding nano-silicon dioxide, cerium salt and phosphate to material A, stirring and standing to obtain material B; (3) Adding alginate, a dispersant, a stabilizer, a bactericide and an auxiliary agent to material B to obtain material C, grinding and sieving material C to obtain the anti-corrosion and anti-fouling coating material.

8. The method for preparing an anticorrosion and antifouling coating material according to claim 7, characterized in that: The stirring rate of the mixing in step (1) is 500-800 rpm, and the mixing time is 8-12 min; In step (2), the stirring rate is 2000-3000 rpm, the stirring time is 4-8 hours, and the standing time is 20-50 minutes.

9. The method for preparing an anti-corrosion and anti-fouling coating material according to claim 8, characterized in that: The stirring rate of the mixing in step (3) is 1500-2500 rpm, and the stirring time is 2-6 hours; The mesh number of the sieving is 120-140 meshes.

10. Use of the anti-corrosion and anti-fouling coating material according to any one of claims 1 to 6 in marine anti-corrosion coatings.

Citation Information

Patent Citations

  • Fluorine-modified zinc acrylate antifouling coating material and preparation method thereof

    CN105295631A

  • Epoxy modified silane marine anti-corrosion and anti-fouling paint

    CN105400419A

  • Peeling antifouling paint of single-component propeller and preparing method thereof

    CN106349928A

  • Thin-coating heavy-duty anticorrosive coating and preparation method thereof

    CN110643267A

  • Metal matrix surface composite coating as well as preparation method and application thereof

    CN117926362A

Cited By

  • Anticorrosive and antibacterial coating composition, anticorrosive and antibacterial coating as well as preparation method and application of anticorrosive and antibacterial coating

    CN121182323A