Forming method of long-axis forge piece
Through the forging of long-axis forgings, the problem of uneven grain size of forgings is solved, and the mechanical properties and safety guarantee of forgings are improved.
Patent Information
- Application Number
- CN202411199330.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-08
AI Technical Summary
Long-axis forgings are prone to poor tissue during the forging process, resulting in uneven grain size and affecting the mechanical properties, especially the grain size of the large head, which affects the mechanical properties of the overall forging.
A forming method is adopted, including cutting to obtain rod-shaped blank, dividing the material into a rod part and a large head molding section, respectively, pulling the length and pier thickness, forming the initial blank, then flattening and then die forging to ensure the large head and The rods are formed evenly to avoid multiple emptying and uneven tissue.
By refining the grains of the large head and rod, the overall grain uniformity of the forging is improved, the mechanical properties are improved, and the stability and safety of the forging is ensured in high-temperature environments.
Smart Images

Figure CN118905127A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of forging, in particular to a forming method for long shaft forgings. Background Art
[0002] Long shaft forgings are key core forgings for aircraft engines. They work for a long time at high temperatures, in harsh working environments, facing complex stress states and bearing alternating loads, so high requirements are placed on the microstructure and mechanical properties of forgings. The manufacturing process of long shaft forgings, especially the forging process, has a great influence on the microstructure and mechanical properties of forgings. Abnormal manufacturing processes are prone to produce undesirable structures, affecting the mechanical level of forgings, thus causing forging failures and major quality and safety accidents. Stable and efficient forging processes and operating methods are the key to the preparation of long shaft high-temperature alloy forgings.
[0003] Long shaft forgings are divided into a large head and a rod. The diameter of the large head is generally greater than φ300mm, the diameter of the rod is generally less than φ150mm, and the total length is greater than 1400mm. Since the diameter of the large head of long shaft forgings is larger than the diameter of conventional bars, in order to ensure the diameter of the large head of the forgings, the forgings are generally made by first upsetting the whole, then dividing the materials, and drawing the blanks, and then the final die forging is performed. However, during the drawing process after upsetting deformation, due to the long rod length of the long shaft forgings, multiple fires are required for drawing. During the entire drawing process, the large head is no longer deformed, that is, it is in a state of multiple fires of empty burning after deformation, and only deforms in the last fire of die forging. In this way, the grains of the large head are coarser, and its surface grain size can only reach 4-5 levels. The grain size of the entire forging is 4-10, and the organization is very uneven, which affects the mechanical properties of the forgings. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a forming method for long-axis forgings which can reduce the grain size of the large head of the forgings, make the grains of the forgings more uniform, and thus improve the mechanical properties of the forgings.
[0005] The technical solution adopted by the present invention to solve the technical problem is: a forming method of a long shaft forging, the forging comprising a rod and a large head arranged at one end of the rod and having a diameter greater than the diameter of the rod, the forming method comprising:
[0006] Cutting according to the size of the forging to obtain a rod-shaped blank;
[0007] After the rough blank is heated, the rough blank is first divided into a rod forming section of the material required for forming the rod and a head forming section of the material required for forming the large head, and then the rod forming section is stretched to form a rod rough blank section according to the rod design, and then the head forming section is roughened to form a large head rough blank section according to the large head design, thereby obtaining a first rough blank;
[0008] Flattening the first preform to obtain a second preform;
[0009] The second preform is die forged to form the forging.
[0010] Furthermore, the blank cutting length l = [φ1×(l1+k)+φ2×(l2+k)]÷φ, wherein φ1 is the diameter of the big head, φ2 is the diameter of the rod, l1 is the length of the big head, l2 is the length of the rod, φ is the diameter of the blank, k is an empirical parameter, and the value range of k is 30 to 100 mm.
[0011] Furthermore, the blank is wrapped with heat-insulating cotton during heating.
[0012] Furthermore, the length of the head forming section is divided according to (l1φ1)÷φ, wherein φ1 is the diameter of the large head, l1 is the length of the large head, and φ is the diameter of the blank.
[0013] Furthermore, the length of the rod blank segment is l2+(10-80) mm, where l2 is the length of the rod.
[0014] Furthermore, the length of the large head blank segment is l1+(30-80) mm, where l1 is the length of the large head.
[0015] Furthermore, the thickness of the stem blank section after being flattened is m1=(0.1-0.5)×φ2mm, and the thickness of the large head blank section after being flattened is m2=(0.4-0.7)φ1mm.
[0016] The beneficial effects of the present invention are as follows: in a forming method of a long shaft forging of the present invention, the forming of the large head blank section is after the forming of the rod blank section 31, thereby avoiding multiple empty burning of the large head blank section 32 and refining the grains of the large head blank section 32. After the large head blank section 32 is roughened, the first blank 3 obtained is flattened to obtain the second blank 4, and finally the second blank 4 is die forged to obtain the forging. In this way, the large head blank section 32 and the rod blank section 31 are also subjected to two extrusion deformations, which increases the deformation of the forging during the forming process, thereby further refining the grains of the rod 11 and the large head 12 of the forging, making the grains of each part of the entire forging more uniform, thereby improving the performance of the forging. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic structural diagram of the forging of the present invention;
[0018] Figure 2 It is a schematic diagram of forging forming of the present invention;
[0019] Figure 3 It is a schematic diagram of the roughening of the head forming section;
[0020] As shown in the figure: forging 1, blank 2, first blank 3, second blank 4, flat anvil 5, support block 6, base 7, rod 11, large head 12, rod forming section 21, head forming section 22, rod blank section 31, large head blank section 32. DETAILED DESCRIPTION
[0021] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0022] like Figure 1 , Figure 2 As shown, a forming method of a long shaft forging of the present invention, the forging 1 includes a rod 11 and a large head 12 disposed at one end of the rod 11 and having a diameter greater than that of the rod 11, the forming method includes:
[0023] Step 1: Cutting the forging 1 according to the size of the forging 1 to obtain a rod-shaped blank 2;
[0024] Step 2: After heating the rough blank 2, the rough blank 2 is first divided into a rod forming section 21 of a material required for forming the rod 11 and a head forming section 22 of a material required for forming the large head 12, and then the rod forming section 21 is stretched to form a rod rough blank section 31 designed according to the rod 11, and then the head forming section 22 is roughened to form a large head rough blank section 32 designed according to the large head 12, thereby obtaining a first rough blank 3;
[0025] Step 3, flattening the first blank 3 to obtain a second blank 4;
[0026] Step 4: placing the second preform 4 into a forging die for die forging to form the forging 1.
[0027] The forming method of the long shaft forging of the present invention is to first stretch the rod forming section 21 of the blank 2 to obtain the rod blank section 31, and then roughen the head forming section 22 of the blank 2 to form a large head blank section 32, and then flatten the formed first blank 3 to obtain the second blank 4, and finally forge the flat second blank 4 to obtain a forging. The large head blank section 32 is formed after the rod blank section 31 is formed, thereby avoiding multiple empty burning of the large head blank section 32 and refining the grains of the large head blank section 32. After the large head blank section 32 is rough-formed, the first blank 3 is flattened to obtain the second blank 4, and finally the second blank 4 is die-forged to obtain a forging. In this way, the large head blank section 32 and the rod blank section 31 will also be extruded and deformed twice, which increases the deformation of the forging during the forming process, thereby further refining the grains of the rod 11 and the large head 12 of the forging, making the grains of each part of the entire forging more uniform, thereby improving the performance of the forging.
[0028] Since the rod of the forging is long, the corresponding rod blank section 31 will also be long. In order to facilitate the roughening of the head forming section 22 of the drawn blank, as shown in FIG. Figure 3 As shown, in the embodiment of the present invention, the roughing adopts a combined tool, including a support block 6 and a base 7 with a hollow interior, the support block 6 is inserted into the inner cavity of the base 7 and supported by the base 7, and the support block 6 is provided with a through hole adapted to the rod blank section 31. When the roughing is short and thick, the rod blank section 31 of the rough is inserted into the through hole of the support block 6, and the surface of the support block cooperates with the end face of the head forming section 22 to support the column rough. When roughing, the head forming section 22 can be short and thickened by squeezing it toward the support block with a flat anvil 5.
[0029] In order to save materials, in the present invention, the blank 2 is preferably cut to a length l = [φ1×(l1+k)+φ2×(l2+k)]÷φ, wherein φ1 is the diameter of the large head 12, φ2 is the diameter of the rod 11, l1 is the length of the large head 12, l2 is the length of the rod 11, φ is the diameter of the blank, and k is an empirical parameter, and the value range of k is 30 to 100 mm. This cutting length can ensure the required forging forming and avoid material waste caused by cutting too long.
[0030] In order to prevent the blank from heating up uniformly during the heating process, it is best to wrap the blank with heat preservation cotton during the heating process. In this way, the blank will heat up slowly, the temperature difference between the inside and the surface of the blank will be small, the blank will heat up more uniformly, the grains will be more uniform, and the performance of the forging will be improved.
[0031] In the best embodiment of the present invention, the length of the head forming section 22 is divided according to (l1φ1)÷φ, wherein φ1 is the diameter of the large head 12, l1 is the length of the large head 12, and φ is the diameter of the blank. The above calculation method is used to divide the materials, which can ensure that the material of the head forming section 22 meets the requirements for forming the large head 12 and the material of the rod forming section 21 meets the requirements for forming the rod 11, and can also avoid the internal structure deformation of the head forming section 22 when it is short and thick due to excessive material. The above method is conducive to refining the grain of the large head of the forging, and can also make the grain of the large head of the forging more uniform.
[0032] In the present invention, the length of the rod blank section 31 is preferably l2+(10-80) mm, where l2 is the length of the rod 11; the length of the large head blank section 32 is l1+(30-80) mm, where l1 is the length of the large head 12. It is more convenient to subsequently die forge when the lengths of the rod blank section 31 and the large head blank section 32 are respectively controlled within the above ranges.
[0033] The thickness of the rod blank section 31 after being flattened and the thickness of the large head blank section 32 after being flattened can be set arbitrarily as needed. In the present invention, in order to make the rod and large head materials of the forging fully deformed after being roughened in the head forming section 22, so that the grains of the forging are finer and more uniform, and at the same time, it is convenient for subsequent die forging, the best thickness of the rod blank section 31 after being flattened is m1 = (0.1 ~ 0.5) × φ2mm, and the thickness of the large head blank section 32 after being flattened is m2 = (0.4 ~ 0.7) φ1mm.
[0034] Embodiment 1:
[0035] The material of forging A is GH4169; the diameter φ1 of the large head 12 is 320 mm, the diameter φ2 of the rod is 120 mm, the length of the large head is l1 = 100 mm, and the length of the rod is l2 = 1400 mm; the forming method of forging 1 is:
[0036] Step 1: Cutting according to the size of the forging 1 to obtain a rod-shaped blank 2, the diameter φ of the rod-shaped blank 2 is 200, and the cutting length of the blank 2 is l = [φ1×(l1+30)+φ2×(l2+30)]÷φ=1066mm;
[0037] Step 2: After heating the blank 2, the blank is first divided into a rod forming section 21 of the material required for forming the rod 11 and a head forming section 22 of the material required for forming the large head 12, and then the rod forming section 21 is stretched to form a rod blank section 31 designed according to the rod 11, and then the head forming section 22 is roughened to form a large head blank section 32 designed according to the large head 12, thereby obtaining a first blank 3, wherein the blank 2 is wrapped with heat-insulating cotton when heated, and the temperature is first raised to 800°C to 900°C during heating, and the heat preservation is Heat for a certain time, at this time, the holding time (min) is based on T1≥(0.8~1.5)×diameterφ of blank 2; then raise the temperature to 990℃~1020℃, and keep it warm for a certain time, at this time, the holding time (min) is based on T2≥(0.7~1.4)×diameterφ of blank 2. The heating in the middle of the drawing process shall be carried out according to the following requirements. For cold parts, that is, forgings with a temperature of <600℃~800℃, wrap them with insulation cotton and put them into the furnace. Put the blank into the furnace for heating, first raise the temperature to 800℃~900℃, and keep it warm for a certain time. At this time, the holding time (min) is based on T n1 ≥(0.8~1.5)×the diameter of the head forming section 22 of the blank at this time; then raise the temperature to 990℃~1020℃, and keep it warm for a certain time. At this time, the warming time (min) is based on T n2 ≥(0.7~1.4)×the diameter of the head forming section 22 of the blank at this time. For hot parts, that is, the forging temperature is greater than 600℃~800℃, the blank is first returned to the furnace to 990℃~1020℃, kept warm for 100min~200min, then taken out of the furnace and wrapped, and then kept warm for more than 60min before being taken out of the furnace for forging. The length of the head forming section 22 is 160mm, the length of the rod blank section 31 is 1410mm, and the length of the large head blank section 32 is 130mm;
[0038] Step 3, flatten the first blank 3 to obtain a second blank 4, wherein the thickness of the rod blank section 31 after flattening is m1=12 mm, and the thickness of the large head blank section 32 after flattening is m2=128 mm;
[0039] Step 4: Place the second blank 4 into a forging die for die forging to form the forging A.
[0040] It was measured that the grain size of the rod part and the grain size of the large head of forging A were both 8-10, and the grain size of the forging was uniform.
[0041] Embodiment 2:
[0042] The material of forging B is GH4169; the diameter φ1 of the large head 12 is 320 mm, the diameter φ2 of the rod is 120 mm, the length of the large head is l1 = 100 mm, and the length of the rod is l2 = 1400 mm; the forming method of forging 2 is:
[0043] Step 1, cutting according to the size of the forging 1 to obtain a rod-shaped blank 2, the diameter φ of the rod-shaped blank 2 is 300, and the cutting length of the blank 2 is l = [φ1×(l1+100)+φ2×(l2+100)]÷φ=1220mm;
[0044] Step 2: After heating the blank 2, the blank is first divided into a rod forming section 21 of the material required for forming the rod 11 and a head forming section 22 of the material required for forming the large head 12, and then the rod forming section 21 is stretched to form a rod blank section 31 designed according to the rod 11, and then the head forming section 22 is roughened to form a large head blank section 32 designed according to the large head 12, thereby obtaining a first blank 3, wherein the blank 2 is wrapped with heat-insulating cotton when heated, and the temperature is first raised to 800°C to 900°C during heating, and the heat preservation is Heat for a certain time, at this time, the holding time (min) is based on T1≥(0.8~1.5)×diameterφ of blank 2; then raise the temperature to 990℃~1020℃, and keep it warm for a certain time, at this time, the holding time (min) is based on T2≥(0.7~1.4)×diameterφ of blank 2. The heating in the middle of the drawing process shall be carried out according to the following requirements. For cold parts, that is, forgings with a temperature of <600℃~800℃, wrap them with insulation cotton and put them into the furnace. Put the blank into the furnace for heating, first raise the temperature to 800℃~900℃, and keep it warm for a certain time. At this time, the holding time (min) is based on T n1 ≥(0.8~1.5)×the diameter of the head forming section 22 of the blank at this time; then raise the temperature to 990℃~1020℃, and keep it warm for a certain time. At this time, the warming time (min) is based on T n2 ≥(0.7~1.4)×the diameter of the head forming section 22 of the blank at this time. For hot parts, that is, the forging temperature is greater than 600℃~800℃, the blank is first returned to the furnace to 990℃~1020℃, kept warm for 100min~200min, then taken out of the furnace and wrapped, and then kept warm for more than 60min before being taken out of the furnace for forging. The length of the head forming section 22 is 160mm, the length of the rod blank section 31 is 1480mm, and the length of the large head blank section 32 is 180mm;
[0045] Step 3, flatten the first blank 3 to obtain a second blank 4, wherein the thickness of the rod blank section 31 after flattening is m1=60mm, and the thickness of the large head blank section 32 after flattening is m2=224mm;
[0046] Step 4: Place the second blank 4 into a forging die for die forging to form the forging B.
[0047] The grain size of the rod part and the grain size of the large head of forging B were measured to be 8-10, and the grain size of the forging was uniform.
Claims
1. A method for forming a long shaft forging, wherein the forging (1) comprises a rod (11) and a large head (12) arranged at one end of the rod (11) and having a diameter greater than that of the rod (11), characterized in that: The molding method comprises: Cutting according to the size of the forging (1) to obtain a rod-shaped blank (2); After the blank (2) is heated, it is first divided into materials to obtain a rod forming section (21) of material required for forming the rod (11) and a head forming section (22) of material required for forming the large head (12), then the rod forming section (21) is stretched to form a rod blank section (31) designed according to the rod (11), and then the head forming section (22) is roughened to form a large head blank section (32) designed according to the large head (12), thereby obtaining a first blank (3); Flattening the first blank (3) to obtain a second blank (4); The second preform (4) is die forged to form the forged part (1).
2. A method for forming a long shaft forging according to claim 1, characterized in that: The blank (2) cutting length l = [φ1×(l1+k)+φ2×(l2+k)]÷φ, wherein φ1 is the diameter of the large head (12), φ2 is the diameter of the rod (11), l1 is the length of the large head (12), l2 is the length of the rod (11), φ is the diameter of the blank, and k is an empirical parameter, the value range of k is 30 to 100 mm.
3. A method for forming a long shaft forging according to claim 1, characterized in that: The blank (2) is wrapped with heat-insulating cotton during the heating process.
4. A method for forming a long shaft forging according to any one of claims 1 to 3, characterized in that: The length of the head forming section (22) is divided according to (l1φ1)÷φ, wherein φ1 is the diameter of the large head (12), l1 is the length of the large head (12), and φ is the diameter of the blank.
5. A method for forming a long shaft forging according to claim 4, characterized in that: The length of the rod blank section (31) is l2+(10-80) mm, where l2 is the length of the rod (11).
6. A method for forming a long shaft forging according to claim 5, characterized in that: The length of the large head blank section (32) is l1+(30-80) mm, where l1 is the length of the large head (12).
7. A method for forming a long shaft forging according to claim 6, characterized in that: The thickness of the rod blank section (31) after being flattened is m1=(0.1-0.5)×φ2mm, and the thickness of the large head blank section (32) after being flattened is m2=(0.4-0.7)φ1mm.
Citation Information
Patent Citations
Precision die forging and shaping technical method for automobile steering knuckle rough type parts
CN102672096A
Forging method for maraging steel disc-shaft integrated forged piece
CN105728631A
Gear shaft product forge piece and machining process thereof
CN109681518A
Die forging forming method and device for GH4169 alloy long-axis forge piece
CN112719175A
Precise blank manufacturing method for large marine connecting rod die forging
CN114535476A