Pouring method for casting reinforcing rib frame

By adopting specific proportions of material mixing and high-frequency vibration casting technology in casting production, combined with air-cooling and heat treatment, the challenges of the casting process to the performance and cost of reinforcement frames are solved, and high-quality and efficient casting production is achieved.

CN118905158APending Publication Date: 2024-11-08SILVER ANHUI FOUNDRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410970345.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the production of existing castings, the casting process affects the performance and quality of the reinforcement frame, and the production cost is high, so it is urgent to improve the quality and production efficiency of the castings.

Method used

A casting method for casting reinforcement frames, including mixing Si, Fe, Mg, Zn, Cu, Ti and composite materials in a specific proportion, melting the electric furnace and pouring on a high-frequency vibration platform, followed by air cooling, surface cutting and heat treatment , finally obtain a finished reinforcement frame product with good strength, elongation and corrosion resistance.

Benefits of technology

It improves the quality and production efficiency of castings, while reducing production costs. The produced reinforced rib frame has excellent tensile strength, elongation and corrosion resistance, and has a broader market prospect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905158A_ABST
    Figure CN118905158A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of casting production, in particular to a pouring method for casting a reinforcing rib frame. According to the method, a reinforcing rib frame mold is placed on a high-frequency vibration platform in advance, then melt of the obtained materials is poured into the reinforcing rib frame mold, after pouring is completed, air cooling is conducted to the room temperature, then surface cutting treatment and heat treatment are conducted, and finally a reinforcing rib frame finished product is obtained. The reinforcing rib frame produced by the invention has good strength, ductility and corrosion resistance; in addition, according to the provided method, the quality and production efficiency of the casting are improved, and meanwhile the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of casting production, in particular to a pouring method for casting a reinforcing rib frame. Background Art

[0002] Pouring is the process of pouring molten metal into a mold to cast metal parts. The role of the reinforcement ribs is not only to improve the strength and rigidity of the product and reduce distortion, but also to make it easier to fill the cavity when the product is formed. Generally, the reinforcement rib frame is cast by pouring.

[0003] The pouring process will affect the performance and quality of the reinforcement frame, as well as the production cost. Therefore, how to effectively improve the pouring process has become an important issue that needs to be solved urgently in my country's casting production industry.

[0004] Therefore, the present invention provides a casting method for a cast reinforcement frame, which is used to solve the above-mentioned related technical problems. Summary of the invention

[0005] The object of the present invention is to provide a casting method for a casting reinforcement frame. The method provided by the present invention and the reinforcement frame produced by the present invention not only have good strength, elongation and corrosion resistance; but also the method provided improves the quality and production efficiency of the casting, while reducing the production cost.

[0006] To achieve the above object, the present invention provides the following technical solutions: The present invention provides a casting method for a casting reinforcement frame, comprising the following steps: S1. Weigh in order by weight: 10-20 parts of Si, 8-10 parts of Fe, 6-10 parts of Mg, 3-7 parts of Zn, 8-12 parts of Cu, 2-6 parts of Ti and 2-4 parts of composite material; S2. Accurately weigh Si, Fe, Mg, Zn, Cu, Ti and the composite material respectively, mix them in a mixing device, and melt the obtained mixture in an electric furnace; S3, placing the rib frame mold on a high-frequency vibration platform in advance, and then pouring the obtained melt into the rib frame mold, and after the pouring is completed, air cooling to room temperature; S4, taking out the reinforcing rib frame casting and performing surface cutting treatment to obtain a reinforcing rib frame casting with a smooth surface; S5, heat treating the obtained reinforcement frame casting; S6. The heat-treated reinforcement frame casting is subjected to inspection and packaging processes in sequence to finally obtain a reinforcement frame finished product.

[0007] The present invention is further configured as follows: in the step S1, the composite material is prepared by mixing Li and Zr in a mass ratio of 0.3 to 0.6:1.

[0008] The present invention is further configured as follows: in step S2, the mixing speed is 120-140 r / min, and the mixing time is 5-10 min.

[0009] The present invention is further configured as follows: in step S2, the melting process is as follows: The first stage: heat the electric furnace to 750-760°C at a heating rate of 6-10°C / min and keep it warm for 20-30 minutes; The second stage: heat the electric furnace to 1440-1480°C at a heating rate of 2-5°C / min and keep it warm for 40-50 minutes.

[0010] The present invention is further configured as follows: in step S3, the vibration frequency of the high-frequency vibration platform is 120-150 Hz, and the amplitude is 0.3 mm.

[0011] The present invention is further configured as follows: in step S3, the pouring process is: The temperature of the melt is controlled at 1250-1300°C, the melt is poured into the rib frame mold, and when the filling rate of the rib frame mold is controlled at 80-85%, the high-frequency vibration platform is stopped; Then slowly pour the remaining melt until the filling rate of the reinforcement frame mold reaches 100%.

[0012] The present invention is further configured as follows: in step S5, the heat treatment process is as follows: The obtained reinforcement frame casting is placed in an electric furnace and heat-treated at 500-520°C for 3-6 hours; Then treat the reinforcement frame casting at -50 to -60°C for 2 to 3 hours; Then the reinforcement frame casting is treated at 140-150°C for 10-12h; Finally, the reinforcement frame casting can be water-cooled.

[0013] The present invention is further configured as follows: the water cooling temperature is 60-70° C. and the time is 120-130 seconds.

[0014] Compared with the prior art, the present invention has the following beneficial effects: The method provided by the present invention is to place the rib frame mold on a high-frequency vibration platform in advance, and then pour the melt of the obtained material into the rib frame mold. After the pouring is completed, it is air-cooled to room temperature, and then surface cutting and heat treatment are performed to finally obtain a rib frame finished product; the rib frame produced by the present invention not only has good strength, elongation and corrosion resistance; but also the method provided improves the quality and production efficiency of the casting, while reducing the production cost. The method provided by the present invention has a broader market prospect and is more suitable for promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 It is a statistical diagram of the tensile strength of the present invention; Figure 2 It is a statistical diagram of the elongation of the present invention; Figure 3 It is a statistical diagram of the weight reduction of the present invention. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] Embodiment 1: This embodiment provides a casting method for a cast reinforcement frame, comprising the following steps: S1. Weigh in order by weight: 10 parts of Si, 8 parts of Fe, 6 parts of Mg, 3 parts of Zn, 8 parts of Cu, 2 parts of Ti and 2 parts of composite material.

[0019] The composite material is prepared by mixing Li and Zr in a mass ratio of 0.3:1.

[0020] S2. Accurately weigh Si, Fe, Mg, Zn, Cu, Ti and the composite material respectively, mix them in a mixing device, and melt the obtained mixture in an electric furnace.

[0021] Furthermore, the mixing speed is 120 r / min and the mixing time is 5 min.

[0022] The melting process is as follows: The first stage: the electric furnace is heated to 750°C at a heating rate of 6°C / min and kept at this temperature for 20 minutes; The second stage: the electric furnace was heated to 1440°C at a heating rate of 2°C / min and kept at this temperature for 40 min.

[0023] S3. Place the rib frame mold on a high-frequency vibration platform in advance, then pour the obtained melt into the rib frame mold, and after the pouring is completed, air cool to room temperature.

[0024] Among them, the vibration frequency of the high-frequency vibration platform is 120 Hz and the amplitude is 0.3 mm.

[0025] The pouring process is: The temperature of the melt is controlled at 1250°C, the melt is poured into the rib frame mold, and when the filling rate of the rib frame mold is controlled to be in the 80% range, the high-frequency vibration platform is stopped; Then slowly pour the remaining melt until the filling rate of the reinforcement frame mold reaches 100%.

[0026] S4, taking out the reinforcing rib frame casting and performing surface cutting treatment to obtain a reinforcing rib frame casting with a smooth surface.

[0027] S5. heat treating the obtained reinforcement frame casting.

[0028] The heat treatment process is as follows: The obtained reinforcement frame casting was placed in an electric furnace and kept at 500°C for 3 hours; Then the reinforcement frame casting was treated at -50°C for 2h; Then the reinforcement frame casting was treated at 140°C for 10 h; Finally, the reinforcement frame casting can be water-cooled.

[0029] Furthermore, the water cooling temperature is 60° C. and the time is 120 s.

[0030] S6. The heat-treated reinforcement frame casting is subjected to inspection and packaging processes in sequence to finally obtain a reinforcement frame finished product.

[0031] Embodiment 2: This embodiment provides a casting method for a cast reinforcement frame, comprising the following steps: S1. Weigh in order by weight: 15 parts of Si, 9 parts of Fe, 8 parts of Mg, 5 parts of Zn, 10 parts of Cu, 4 parts of Ti and 3 parts of composite material.

[0032] The composite material is prepared by mixing Li and Zr in a mass ratio of 0.4:1.

[0033] S2. Accurately weigh Si, Fe, Mg, Zn, Cu, Ti and the composite material respectively, mix them in a mixing device, and melt the obtained mixture in an electric furnace.

[0034] Furthermore, the mixing speed is 130 r / min and the mixing time is 7 min.

[0035] The melting process is as follows: Stage 1: Heat the furnace to 755°C at a heating rate of 8°C / min and keep it at that temperature for 25 minutes; The second stage: heat the electric furnace to 1460°C at a heating rate of 2-5°C / min and keep it at that temperature for 45 minutes.

[0036] S3. Place the rib frame mold on a high-frequency vibration platform in advance, then pour the obtained melt into the rib frame mold, and after the pouring is completed, air cool to room temperature.

[0037] Among them, the vibration frequency of the high-frequency vibration platform is 135Hz and the amplitude is 0.3mm.

[0038] The pouring process is: The temperature of the melt is controlled at 1275°C, the melt is poured into the rib frame mold, and when the filling rate of the rib frame mold is controlled to be in the range of 82%, the high-frequency vibration platform is stopped; Then slowly pour the remaining melt until the filling rate of the reinforcement frame mold reaches 100%.

[0039] S4, taking out the reinforcing rib frame casting and performing surface cutting treatment to obtain a reinforcing rib frame casting with a smooth surface.

[0040] S5. heat treating the obtained reinforcement frame casting.

[0041] The heat treatment process is as follows: The obtained reinforcement frame casting was placed in an electric furnace and kept at 510°C for 4 hours; Then the reinforcement frame casting was treated at -55°C for 2h; Then the reinforcement frame casting was treated at 145°C for 11 h; Finally, the reinforcement frame casting can be water-cooled.

[0042] Furthermore, the water cooling temperature is 65° C. and the time is 125 s.

[0043] S6. The heat-treated reinforcement frame casting is subjected to inspection and packaging processes in sequence to finally obtain a reinforcement frame finished product.

[0044] Embodiment 3: This embodiment provides a casting method for a cast reinforcement frame, comprising the following steps: S1. Weigh in order by weight: 20 parts of Si, 10 parts of Fe, 10 parts of Mg, 7 parts of Zn, 12 parts of Cu, 6 parts of Ti and 4 parts of composite material.

[0045] The composite material is prepared by mixing Li and Zr in a mass ratio of 0.6:1.

[0046] S2. Accurately weigh Si, Fe, Mg, Zn, Cu, Ti and the composite material respectively, mix them in a mixing device, and melt the obtained mixture in an electric furnace.

[0047] Furthermore, the mixing speed is 140 r / min and the mixing time is 10 min.

[0048] The melting process is as follows: The first stage: the electric furnace is heated to 760°C at a heating rate of 10°C / min and kept at this temperature for 30 minutes; The second stage: the electric furnace was heated to 1480°C at a heating rate of 5°C / min and kept at this temperature for 50 min.

[0049] S3. Place the rib frame mold on a high-frequency vibration platform in advance, then pour the obtained melt into the rib frame mold, and after the pouring is completed, air cool to room temperature.

[0050] Among them, the vibration frequency of the high-frequency vibration platform is 150 Hz and the amplitude is 0.3 mm.

[0051] The pouring process is: The temperature of the melt is controlled at 1300°C, the melt is poured into the rib frame mold, and when the filling rate of the rib frame mold is controlled to be in the range of 85%, the high-frequency vibration platform is stopped; Then slowly pour the remaining melt until the filling rate of the reinforcement frame mold reaches 100%.

[0052] S4, taking out the reinforcing rib frame casting and performing surface cutting treatment to obtain a reinforcing rib frame casting with a smooth surface.

[0053] S5. heat treating the obtained reinforcement frame casting.

[0054] The heat treatment process is as follows: The obtained reinforcement frame casting was placed in an electric furnace and kept at 520°C for 6 hours; Then the reinforcement frame casting was treated at -60°C for 3h; Then the reinforcement frame casting was treated at 150°C for 12 h; Finally, the reinforcement frame casting can be water-cooled.

[0055] Furthermore, the water cooling temperature is 70° C. and the time is 130 s.

[0056] S6. The heat-treated reinforcement frame casting is subjected to inspection and packaging processes in sequence to finally obtain a reinforcement frame finished product.

[0057] Effect test The reinforced rib frames prepared by Examples 1 to 3 of the present invention are respectively recorded as Experimental Examples 1 to 3; and then the performance of each group of reinforced rib frame samples is tested respectively.

[0058] Test 1. Mechanical properties test and result analysis: The tensile strength and elongation of the reinforced rib frame were measured according to the method for measuring the tensile strength and elongation of the reinforced rib frame in GB / T228-2010. The relevant data are recorded in Table 1.

[0059] Table 1: Test data record table

[0060] From Table 1 and Figure 1-2 It can be seen that the reinforced rib frames of Examples 1 to 3 have excellent tensile strength and elongation, and at the same time, the differences between the example groups are not obvious; the method provided by the present invention can effectively improve the mechanical properties of the reinforced rib frame.

[0061] Test 2: Corrosion resistance test and result analysis: After grinding the sample with sandpaper, the sample was made and subjected to ASTM A262 test and salt spray test. The relevant data are recorded in Table 2.

[0062] Table 2: Test data record table

[0063] From Table 2 and Figure 3 It can be seen that the reinforced rib frames of Examples 1 to 3 have excellent corrosion resistance, and at the same time, the differences between the example groups are not obvious; the reinforced rib frame produced by the method provided by the present invention has excellent corrosion resistance.

[0064] From the above, it can be seen that the reinforced rib frame produced by the present invention not only has good strength, elongation and corrosion resistance, but also improves the quality and production efficiency of castings and reduces production costs. This shows that the method provided by the present invention has a broader market prospect and is more suitable for promotion.

[0065] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0066] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A casting method for a casting reinforcement frame, characterized in that: The following steps are involved: S1. Weigh in order by weight: 10-20 parts of Si, 8-10 parts of Fe, 6-10 parts of Mg, 3-7 parts of Zn, 8-12 parts of Cu, 2-6 parts of Ti and 2-4 parts of composite material; S2. Accurately weigh Si, Fe, Mg, Zn, Cu, Ti and the composite material respectively, mix them in a mixing device, and melt the obtained mixture in an electric furnace; S3, placing the rib frame mold on a high-frequency vibration platform in advance, and then pouring the obtained melt into the rib frame mold, and after the pouring is completed, air cooling to room temperature; S4, taking out the reinforcement frame casting and performing surface cutting treatment to obtain a reinforcement frame casting with a smooth surface; S5, heat treating the obtained reinforcement frame casting; S6. The heat-treated reinforcement frame casting is subjected to inspection and packaging processes in sequence to finally obtain a reinforcement frame finished product.

2. A method for casting a reinforcement frame according to claim 1, characterized in that: In the step S1, the composite material is prepared by mixing Li and Zr in a mass ratio of 0.3 to 0.6:

1.

3. A casting method for a reinforcement frame according to claim 1, characterized in that: In the step S2, the mixing speed is 120-140 r / min, and the mixing time is 5-10 min.

4. A method for casting a reinforcement frame according to claim 1, characterized in that: In step S2, the melting process is as follows: The first stage: heat the electric furnace to 750-760°C at a heating rate of 6-10°C / min and keep it warm for 20-30 minutes; The second stage: heat the electric furnace to 1440-1480°C at a heating rate of 2-5°C / min and keep it warm for 40-50 minutes.

5. A method for casting a reinforcement frame according to claim 1, characterized in that: In step S3, the vibration frequency of the high-frequency vibration platform is 120-150 Hz, and the amplitude is 0.3 mm.

6. A method for casting a reinforcement frame according to claim 1, characterized in that: In step S3, the pouring process is: The temperature of the melt is controlled at 1250-1300°C, the melt is poured into the rib frame mold, and when the filling rate of the rib frame mold is controlled at 80-85%, the high-frequency vibration platform is stopped; Then slowly pour the remaining melt until the filling rate of the reinforcement frame mold reaches 100%.

7. A method for casting a reinforcement frame according to claim 1, characterized in that: In step S5, the heat treatment process is as follows: The obtained reinforcement frame casting is placed in an electric furnace and heat-treated at 500-520°C for 3-6 hours; Then treat the reinforcement frame casting at -50 to -60°C for 2 to 3 hours; Then the reinforcement frame casting is treated at 140-150°C for 10-12h; Finally, the reinforcement frame casting can be water-cooled.

8. A method for casting a reinforcement frame according to claim 7, characterized in that: The water cooling temperature is 60-70° C. and the time is 120-130 seconds.