Aluminum alloy low-temperature diffusion welding method and aluminum alloy welding joint

Through the self-nanization of aluminum alloy base material and electric field heating in SPS diffusion welding equipment, the problems of large energy consumption and easy blockage of microflowers during aluminum alloy welding are solved, and low-temperature and high-quality connections are achieved.

CN118905407APending Publication Date: 2024-11-08HARBIN INST OF TECH
View PDF 0 Cites 7 Cited by

Patent Information

Application Number
CN202411156781.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The problem of high energy consumption and easy blockage of microflow channels during diffusion welding of aluminum alloys.

Method used

By self-nanoization of the surface of the aluminum alloy base material, a nanostructure layer is formed, and an electric field is applied to the SPS diffusion welding equipment to achieve low temperature heating, avoiding the plastic deformation of the base material and microflower blockage caused by the growth of nanocrystals.

Benefits of technology

The welding temperature and energy consumption are reduced, the high diffusion coefficient of the nanostructured layer is maintained, and high-quality aluminum alloy connection is achieved under low temperature conditions, avoiding microflower blockage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905407A_ABST
    Figure CN118905407A_ABST
Patent Text Reader

Abstract

The invention provides an aluminum alloy low-temperature diffusion welding method and an aluminum alloy welding joint, and relates to the technical field of metal connection. The aluminum alloy low-temperature diffusion welding method comprises the steps that the surfaces of aluminum alloy base materials are subjected to self-nanocrystallization, a middle layer is arranged between the two aluminum alloy base materials with nanostructure layers formed on the surfaces, and a to-be-welded piece is obtained; and the to-be-welded part is placed in diffusion welding equipment to be welded, an electric field is applied to the diffusion welding equipment, low-temperature welding is conducted, and the aluminum alloy welded joint is obtained. The surface of the aluminum alloy base material is subjected to self-nanocrystallization to form the nanostructure layer, the nanostructure layer has the advantages of being high in surface energy, low in melting point, high in diffusion coefficient and the like, an electric field applied in diffusion welding equipment can be rapidly heated, nanocrystals of the nanostructure layer are prevented from growing, and the advantage that the diffusion coefficient of the nanostructure layer is high can be kept; and diffusion is promoted through the high diffusion coefficient of the nano-structure layer, and high-quality connection of the aluminum alloy is achieved under the low-temperature condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal connection, and in particular to an aluminum alloy low-temperature diffusion welding method and an aluminum alloy welding joint. Background Art

[0002] The main manufacturing method for microfluidic heat dissipation structures containing microchannels in aluminum alloys is diffusion welding. At present, diffusion welding often requires a long time under high temperature and high pressure to achieve high-strength connection of high-temperature alloys, which consumes a lot of energy. However, in the process of forming high-strength joints, the parent material often undergoes severe plastic deformation, which will cause blockage of the microchannels. Summary of the invention

[0003] The problem solved by the invention is how to solve the problem of high energy consumption of aluminum alloy diffusion welding and easy clogging of micro-channels.

[0004] In order to solve the above problems, the present invention provides an aluminum alloy low-temperature diffusion welding method and an aluminum alloy welding joint.

[0005] In a first aspect, the present invention provides a method for low temperature diffusion welding of aluminum alloys, comprising the following steps:

[0006] S1: performing self-nano treatment on the surface of the aluminum alloy base material to form a nanostructured layer on the surface of the aluminum alloy base material;

[0007] S2: an intermediate layer is arranged between two aluminum alloy base materials with nanostructured layers formed on their surfaces, wherein the intermediate layer contacts the nanostructured layers of the two aluminum alloy base materials to obtain a weldment;

[0008] S3: placing the workpiece to be welded in a diffusion welding device for welding, applying an electric field in the diffusion welding device so that the heating rate of the workpiece to be welded is 20-120°C / min, the welding temperature is 400-500°C, and cooling is performed after welding to obtain an aluminum alloy welded joint.

[0009] Optionally, step S1 specifically includes: placing the aluminum alloy base material in an ultrasonic shot peening device, and shot peening the surface of the aluminum alloy base material to perform self-nano-chemical treatment, so that a nanostructured layer is formed on the surface of the aluminum alloy base material.

[0010] Optionally, in the shot peening treatment, the projectiles used are zirconia ceramics with a diameter of 3 mm, the shot peening distance is 8-12 mm, and the shot peening time is 15-30 min.

[0011] Optionally, the diffusion welding equipment is an SPS diffusion welding equipment, and a pulse electric field is applied in the SPS diffusion welding equipment.

[0012] Optionally, the vacuum degree in the diffusion welding equipment is 10 -1 -10 -2Pa, welding pressure is 5MPa, and welding insulation time is 150min.

[0013] Optionally, before the self-nano-processing, the surface of the aluminum alloy base material is polished with sandpaper, then ultrasonically cleaned in acetone, and dried.

[0014] Optionally, between step S1 and step S2, the following step is further included: immersing the aluminum alloy base material and the intermediate layer in a NaOH solution for alkaline washing, placing them in acetone for ultrasonic cleaning after the alkaline washing, and then immersing them in a HNO3 solution for acid washing, and placing them in acetone for ultrasonic cleaning after the acid washing to obtain a clean aluminum alloy base material and the intermediate layer.

[0015] Optionally, the middle layer is 1060 aluminum alloy.

[0016] Optionally, the aluminum alloy base material is 5A06 aluminum alloy.

[0017] In a second aspect, the present invention provides an aluminum alloy welded joint, which is made by the aluminum alloy low-temperature diffusion welding method as described in any one of the above items.

[0018] The beneficial effects of the aluminum alloy low-temperature diffusion welding method and the aluminum alloy welding joint of the present invention are as follows: the surface of the aluminum alloy base material undergoes self-nanoization, so that a nanostructured layer is formed on the surface of the aluminum alloy base material. The nanostructured layer has the advantages of high surface energy, low melting point, high diffusion coefficient, etc., and can be applied to diffusion welding and reduce the welding temperature to 400-500°C, thereby reducing the energy consumption required for diffusion welding. However, during the heating process of diffusion welding, the nanocrystals of the nanostructured layer often grow and lose the advantage of a high diffusion coefficient.

[0019] Therefore, the electric field applied in the diffusion welding equipment can be used for rapid heating, so that the heating rate is specifically 80-120℃ / min, so as to avoid the growth of nanocrystals in the nanostructure layer, and further avoid the problem of microchannel blockage caused by severe plastic deformation of the base material due to the growth of nanocrystals. At the same time, the advantage of the high diffusion coefficient of the nanostructure layer can be maintained, and the high diffusion coefficient of the nanostructure layer can be used to promote diffusion, so as to achieve high-quality connection of aluminum alloys at low temperatures of 400-500℃. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a flow chart of the aluminum alloy low temperature diffusion welding method of this embodiment;

[0021] Figure 2 This is the microstructure diagram of the aluminum alloy welded joint obtained by the aluminum alloy low-temperature diffusion welding method in Example 1.

[0022] Figure 3 This is the microstructure diagram of the aluminum alloy welded joint obtained by the aluminum alloy low-temperature diffusion welding method in Comparative Example 1. DETAILED DESCRIPTION

[0023] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.

[0024] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;

[0025] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.

[0026] In the related art, 5A06 aluminum alloy is an Al-Mg aluminum alloy, which has the advantages of light weight, corrosion resistance and high strength, and is often used in microchannel heat dissipation structures.

[0027] SPS (Spark Plasma Sintering) diffusion welding is an efficient welding method that uses the material's own resistance and interface contact resistance to quickly heat the interface to be connected and achieve metallurgical bonding of the interface under a certain pressure and time. SPS welding only heats the interface, while the temperature away from the interface is lower, so it can avoid deformation of the parent material and grain coarsening, and at the same time can speed up welding efficiency. This method has the advantages of fast heating rate, low connection temperature, short connection time, and low energy consumption.

[0028] Nanocrystalline layers have the advantages of high surface energy, low melting point, and high diffusion coefficient, and can be used in diffusion welding and reduce welding temperature. However, due to the high surface energy of nanocrystalline itself, they often grow and lose the advantage of high diffusion coefficient during the heating process of diffusion welding.

[0029] Therefore, the present invention adopts shot peening for surface nano-processing combined with SPS technology to perform diffusion welding on 5A06 aluminum alloy, utilizes the rapid heating of SPS heating to avoid the growth of nanocrystals, and utilizes the high diffusion coefficient of nanocrystals to promote diffusion, thereby achieving high-quality connection of 5A06 aluminum alloy under low temperature and small deformation conditions.

[0030] In view of the problems existing in the above-mentioned related technologies, this embodiment provides an aluminum alloy low-temperature diffusion welding method and an aluminum alloy welding joint.

[0031] like Figure 1 As shown, an aluminum alloy low temperature diffusion welding method provided by an embodiment of the present invention comprises the following steps:

[0032] S1: performing self-nano treatment on the surface of the aluminum alloy base material to form a nanostructured layer on the surface of the aluminum alloy base material;

[0033] S2: an intermediate layer is arranged between two aluminum alloy base materials with nanostructured layers formed on their surfaces, wherein the intermediate layer contacts the nanostructured layers of the two aluminum alloy base materials to obtain a weldment;

[0034] S3: placing the workpiece to be welded in a diffusion welding device for welding, applying an electric field in the diffusion welding device so that the heating rate of the workpiece to be welded is 80-120°C / min, the welding temperature is 400-500°C, and cooling is performed after welding to obtain an aluminum alloy welded joint.

[0035] In the present embodiment, the surface of the aluminum alloy base material is self-nano-tized to form a nanostructured layer on the surface of the aluminum alloy base material. The nanostructured layer has the advantages of high surface energy, low melting point, and high diffusion coefficient. It can be applied to diffusion welding and reduce the welding temperature to 400-500°C, thereby reducing the energy consumption required for diffusion welding. However, during the heating process for diffusion welding, the nanocrystals of the nanostructured layer often grow and lose the advantage of a high diffusion coefficient. Therefore, the electric field applied in the diffusion welding equipment can be used for rapid heating, so that the heating rate is specifically 80-120°C / min to avoid the growth of nanocrystals of the nanostructured layer, thereby avoiding the problem of microchannel blockage caused by severe plastic deformation of the base material caused by the growth of nanocrystals. At the same time, the advantage of the high diffusion coefficient of the nanostructured layer can be maintained, and the high diffusion coefficient of the nanostructured layer is used to promote diffusion, thereby achieving high-quality connection of aluminum alloys at low temperatures of 400-500°C.

[0036] Optionally, step S1 specifically includes: placing the aluminum alloy base material in an ultrasonic shot peening device, and shot peening the surface of the aluminum alloy base material to perform self-nano-chemical treatment, so that a nanostructured layer is formed on the surface of the aluminum alloy base material.

[0037] In this optional embodiment, shot peening is used to self-nano-ize the surface of the aluminum alloy base material, so that a nanostructured layer is formed on the surface of the aluminum alloy base material. The nanostructured layer has the advantages of high surface energy, low melting point, and high diffusion coefficient, and can be applied to diffusion welding and reduce the welding temperature.

[0038] Optionally, in the shot peening treatment, the projectiles used are zirconia ceramics with a diameter of 3 mm, the shot peening distance is 8-12 mm, and the shot peening time is 15-30 min.

[0039] In this optional embodiment, the surface of the aluminum alloy base material can be self-nano-chemically processed to form nanocrystals on the surface of the aluminum alloy base material.

[0040] Alternatively, nanocrystals may be prepared on the surface of the aluminum alloy base material by mechanical grinding.

[0041] Specifically, the mechanical grinding pressing depth is 0.05-0.2 mm, the machine tool speed is 200-2000 r / min, and the feed speed is 20-100 mm / min.

[0042] Optionally, the diffusion welding equipment is an SPS diffusion welding equipment, and a pulse electric field is applied in the SPS diffusion welding equipment.

[0043] In this optional embodiment, SPS (spark plasma sintering) diffusion welding is a highly efficient welding method that utilizes the material's own resistance and interface contact resistance to rapidly heat the interface being connected and achieve metallurgical bonding of the interface under a certain pressure and time. SPS welding only heats the interface, while the temperature of the area away from the interface is relatively low, thereby avoiding deformation of the parent material and grain coarsening, and at the same time accelerating welding efficiency. This method has the advantages of fast heating rate, low connection temperature, short connection time, and low energy consumption.

[0044] Optionally, the vacuum degree in the diffusion welding equipment is 10 -1 -10 -2 Pa, welding pressure is 5MPa, and welding insulation time is 150min.

[0045] In this optional embodiment, the electric field applied in the diffusion welding equipment can be used to quickly heat the nanocrystals in the nanostructure layer to avoid the growth of nanocrystals in the nanostructure layer. The high diffusion coefficient of the nanostructure layer can be maintained, and the high diffusion coefficient of the nanostructure layer is used to promote diffusion. The welding can be completed in 150 minutes, and high-quality connection of aluminum alloys can be quickly achieved with high welding efficiency.

[0046] Specifically, direct current or other power sources can also be applied to the diffusion welding equipment, and the current density is controlled at 3A / mm 2 -10A / mm 2 .

[0047] Optionally, before the self-nano-processing, the surface of the aluminum alloy base material is polished with sandpaper, then ultrasonically cleaned in acetone, and dried.

[0048] Specifically, the surface of the aluminum alloy base material was polished using sandpapers of 80 mesh, 600 mesh, 1500 mesh, and 3000 mesh.

[0049] Optionally, between step S1 and step S2, the following step is further included: immersing the aluminum alloy base material and the intermediate layer in a NaOH solution for alkaline washing, placing them in acetone for ultrasonic cleaning after the alkaline washing, and then immersing them in a HNO3 solution for acid washing, and placing them in acetone for ultrasonic cleaning after the acid washing to obtain a clean aluminum alloy base material and the intermediate layer.

[0050] In this optional embodiment, alkali washing is performed to remove oily dirt and oxide film (such as Al2O3) on the surface of the aluminum alloy base material, and acid washing is performed to remove residual reactants after alkali washing.

[0051] Optionally, the middle layer is 1060 aluminum alloy.

[0052] In this optional embodiment, the thickness of the 1060 aluminum alloy is in the range of 10-200 microns, and the joint welding quality increases with the thickness; the diameter of the 1060 aluminum alloy is 20-120 mm.

[0053] Optionally, the aluminum alloy is 5A06 aluminum alloy.

[0054] In this optional embodiment, 5A06 aluminum alloy is an Al-Mg aluminum alloy, which has the advantages of being light, corrosion-resistant and high in strength, and is commonly used in microchannel heat dissipation structures. Specifically, the thickness of 5A06 aluminum alloy is 5-100 mm.

[0055] An aluminum alloy welded joint provided in an embodiment of the present invention is manufactured by using the aluminum alloy low-temperature diffusion welding method as described in any one of the above items.

[0056] Specifically, Figure 2 As shown, the aluminum alloy welded joint is well bonded and has no obvious holes.

[0057] The present invention is further described below in conjunction with specific embodiments.

[0058] Example 1: Aluminum alloy low temperature diffusion welding method based on surface self-nano-crystallization and electric field

[0059] (1) The surface of 5A06 aluminum alloy was polished using 80 mesh, 600 mesh, 1500 mesh, and 3000 mesh sandpaper, and then ultrasonically cleaned in acetone for 30 min, and then dried for later use;

[0060] (2) The polished 5A06 aluminum alloy with a diameter of 53 mm was placed in an ultrasonic shot peening device, the shot was a zirconia ceramic with a diameter of 3 mm, the shot peening distance was 10 mm, and the shot peening time was 20 min;

[0061] (3) The shot-peened 5A06 aluminum alloy and the 12 μm thick 1060 aluminum intermediate layer were immersed in a 10% NaOH solution and alkaline washed for 5 min. After alkaline washing, they were ultrasonically cleaned in acetone for 8 min.

[0062] (4) immersing the 5A06 aluminum alloy and the 1060 aluminum intermediate layer after alkali washing in a 20% HNO3 solution, pickling for 8 minutes, and then ultrasonically cleaning in acetone for 30 minutes;

[0063] (5) A 12 μm thick 1060 aluminum intermediate layer was placed between two pieces of 5A06 aluminum alloy after shot peening, and then placed in an SPS diffusion welding device for welding. The vacuum degree of the SPS diffusion welding device was 10 -1 Pa. During the welding process, the heating rate is 100℃ / min, the welding temperature is 460℃, the pressure is 5MPa, the holding time is 150min, and then the welded parts are cooled in the furnace. After cooling, they are taken out and finally a high-quality 5A06 aluminum alloy welded joint with low temperature and small deformation is obtained. Figure 2 As shown, the aluminum alloy welded joint is well bonded and has no obvious holes.

[0064] Example 2: Aluminum alloy low temperature diffusion welding method based on surface self-nano-crystallization and electric field

[0065] (1) The surface of 5A06 aluminum alloy was polished using 80 mesh, 600 mesh, 1500 mesh, and 3000 mesh sandpaper, and then ultrasonically cleaned in acetone for 30 min, and then dried for later use;

[0066] (2) The polished 5A06 aluminum alloy with a diameter of 53 mm was placed in an ultrasonic shot peening device, the shot was a zirconia ceramic with a diameter of 3 mm, the shot peening distance was 8 mm, and the shot peening time was 15 min;

[0067] (3) The shot-peened 5A06 aluminum alloy and the 12 μm thick 1060 aluminum intermediate layer were immersed in a 10% NaOH solution and alkaline washed for 5 min. After alkaline washing, they were ultrasonically cleaned in acetone for 5 min.

[0068] (4) immersing the 5A06 aluminum alloy and the 1060 aluminum intermediate layer after alkali washing in a 20% HNO3 solution, pickling for 5 minutes, and then ultrasonically cleaning in acetone for 30 minutes;

[0069] (5) A 12 μm thick 1060 aluminum intermediate layer was placed between two pieces of 5A06 aluminum alloy after shot peening, and then placed in an SPS diffusion welding device for welding. The vacuum degree of the SPS diffusion welding device was 10 -1 Pa. During the welding process, the heating rate is 80℃ / min, the welding temperature is 400℃, the pressure is 5MPa, the holding time is 150min, and then the welded parts are cooled in the furnace. After cooling, they are taken out, and finally a high-quality 5A06 aluminum alloy welded joint with low temperature and small deformation is obtained. The obtained aluminum alloy welded joint is also as in Example 1, with good bonding and no obvious holes.

[0070] Example 3: Aluminum alloy low temperature diffusion welding method based on surface self-nano-crystallization and electric field

[0071] (1) The surface of 5A06 aluminum alloy was polished using 80 mesh, 600 mesh, 1500 mesh, and 3000 mesh sandpaper, and then ultrasonically cleaned in acetone for 30 min, and then dried for later use;

[0072] (2) The polished 5A06 aluminum alloy with a diameter of 53 mm was placed in an ultrasonic shot peening device, the shot was a zirconia ceramic with a diameter of 3 mm, the shot peening distance was 12 mm, and the shot peening time was 30 min;

[0073] (3) The shot-peened 5A06 aluminum alloy and the 12 μm thick 1060 aluminum intermediate layer were immersed in a 10% NaOH solution and alkaline washed for 5 min. After alkaline washing, they were ultrasonically cleaned in acetone for 10 min.

[0074] (4) immersing the 5A06 aluminum alloy and the 1060 aluminum intermediate layer after alkali washing in a 20% HNO3 solution, pickling for 10 minutes, and then ultrasonically cleaning in acetone for 30 minutes;

[0075] (5) A 12 μm thick 1060 aluminum intermediate layer was placed between two pieces of 5A06 aluminum alloy after shot peening, and then placed in an SPS diffusion welding device for welding. The vacuum degree of the SPS diffusion welding device was 10 -2 Pa. During the welding process, the heating rate is 120℃ / min, the welding temperature is 500℃, the pressure is 5MPa, the holding time is 150min, and then the welded parts are cooled in the furnace. After cooling, they are taken out, and finally a high-quality 5A06 aluminum alloy welded joint with low temperature and small deformation is obtained. The obtained aluminum alloy welded joint is also as in Example 1, with good bonding and no obvious holes.

[0076] Comparative Example 1, 5A06 aluminum alloy diffusion welding method

[0077] (1) The surface of 5A06 aluminum alloy was polished using 80 mesh, 600 mesh, 1500 mesh, and 3000 mesh sandpaper, and then ultrasonically cleaned in acetone for 30 min, and then dried for later use;

[0078] (2) The 5A06 aluminum alloy and the 1060 aluminum intermediate layer with a thickness of 12 μm were immersed in a 10% NaOH solution and alkaline washed for 5 min. After alkaline washing, they were ultrasonically cleaned in acetone for 10 min.

[0079] (3) immersing the 5A06 aluminum alloy and the 1060 aluminum intermediate layer after alkali washing in a 20% HNO3 solution, pickling for 10 minutes, and then ultrasonically cleaning in acetone for 30 minutes;

[0080] (4) A 12 μm thick 1060 aluminum intermediate layer was placed between two pieces of 5A06 aluminum alloy and welded in an SPS diffusion welding device with a vacuum degree of 10 -2 Pa. During the welding process, the heating rate is 100℃ / min, the welding temperature is 500℃, the pressure is 5MPa, and the holding time is 150min. The welded parts are then cooled in the furnace. After cooling, the welded parts are taken out and the obtained aluminum alloy welded joints are as follows: Figure 3 As shown, the bonding surface is obvious and there are obvious holes.

[0081] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A low temperature diffusion welding method for aluminum alloy, characterized in that: The following steps are involved: S1: performing self-nano treatment on the surface of the aluminum alloy base material to form a nanostructured layer on the surface of the aluminum alloy base material; S2: Arranging an intermediate layer between the two aluminum alloy base materials with nanostructured layers formed on their surfaces, wherein the intermediate layer contacts the nanostructured layers of the two aluminum alloy base materials, to obtain a weldment; S3: placing the workpiece to be welded in a diffusion welding device for welding, applying an electric field in the diffusion welding device to make the heating rate of the workpiece to be welded be 80-120°C / min, the welding temperature be 400-500°C, cooling after welding to obtain an aluminum alloy welded joint.

2. The aluminum alloy low temperature diffusion welding method according to claim 1, characterized in that: The step S1 specifically includes: placing the aluminum alloy base material in an ultrasonic shot peening device, and shot peening the surface of the aluminum alloy base material to perform self-nano-chemical treatment, so that the nanostructured layer is formed on the surface of the aluminum alloy base material.

3. The aluminum alloy low temperature diffusion welding method according to claim 2, characterized in that: In the shot peening treatment, the projectiles used are zirconia ceramics with a diameter of 3 mm, the shot peening distance is 8-12 mm, and the shot peening time is 15-30 minutes.

4. The aluminum alloy low temperature diffusion welding method according to claim 1, characterized in that: The diffusion welding equipment is an SPS diffusion welding equipment, and a pulse electric field is applied in the SPS diffusion welding equipment.

5. The aluminum alloy low temperature diffusion welding method according to claim 1, characterized in that: The degree of vacuum in the diffusion welding equipment is 10 -1 -10 -2 Pa, welding pressure is 5MPa, and welding insulation time is 150min.

6. The aluminum alloy low temperature diffusion welding method according to claim 1, characterized in that: Before the surface of the aluminum alloy base material is subjected to self-nano treatment, the surface of the aluminum alloy base material is polished with sandpaper, and then ultrasonically cleaned in acetone and dried.

7. The aluminum alloy low temperature diffusion welding method according to claim 1, characterized in that: The step between step S1 and step S2 also includes: immersing the aluminum alloy base material and the intermediate layer in a NaOH solution for alkaline washing, placing them in acetone for ultrasonic cleaning after alkaline washing, and then immersing them in a HNO3 solution for acid washing, and placing them in acetone for ultrasonic cleaning after acid washing to obtain the clean aluminum alloy base material and the intermediate layer.

8. The aluminum alloy low temperature diffusion welding method according to claim 1, characterized in that: The middle layer is 1060 aluminum alloy.

9. The aluminum alloy low temperature diffusion welding method according to claim 1, characterized in that: The aluminum alloy base material is 5A06 aluminum alloy.

10. An aluminum alloy welded joint, characterized in that: The aluminum alloy is manufactured by the aluminum alloy low-temperature diffusion welding method as described in any one of claims 1 to 9.

Citation Information

Cited By

  • Magnesium alloy welding method and joint based on semi-solid intermediate layer and pulse current

    CN119549823A

  • Aluminum alloy welding method, aluminum alloy structural part and vehicle

    CN119952227A

  • Method for rapid diffusion bonding of discharge plasma after ultrasonic impact surface treatment

    CN120839428A

  • Small-deformation and high-strength solid-phase diffusion welding method for aluminum alloy

    CN121156471A

  • Aluminum alloy solid phase diffusion welding method with small deformation and high strength

    CN121156471B