Welding material and welding method for welding alloy steel

Through welding wire and laser wire fill welding technology composed of specific elements, the problems of liquid metal embrittlement and porous trachoma in welding ultra-high strength steel are solved, and high-quality welding, material structural uniformity after welding, and weld and parent material are achieved. Performance matching, high welding yield.

CN118905498APending Publication Date: 2024-11-08江苏大族智能焊接装备集团有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410563825.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing welding technology is prone to liquid metal embrittlement and porous trachoma problems when welding ultra-high strength steel, resulting in low welding quality and difficulty in effectively welding stainless steel and hot stamped steel plates.

Method used

Welding wire composed of specific elements is used to weld ultra-high strength steel through laser wire fill welding technology, adjust the proportion and form of the wire element, and combine post-weld heat treatment to form high-quality welds.

Benefits of technology

The welding quality and mechanical strength are improved, the sensitivity to plating is reduced, and the welding effect is achieved with a high yield. The material structure after welding is more uniform and consistent. The weld and the base material performance are matched, and the welding yield can reach 99.99%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905498A_ABST
    Figure CN118905498A_ABST
Patent Text Reader

Abstract

According to the welding material for welding the alloy steel and the welding method, the material welded through the welding material can still keep high mechanical strength and regularity, the tensile strength of the material can reach up to 1546 MPa and is equivalent to that of the alloy steel before welding, and the regular plastic extension strength Rp0.2 of the material reaches up to 1109 MPa. And according to the welding method, a new and integrated structure is formed between the materials, so that the welding seam and the base metal are well matched in performance, and the quality of the welding seam is improved. Besides, dissimilar steel welding of the stainless steel welding wire and the hot stamping forming steel plate is achieved by regulating and controlling the element composition and proportion of the welding wire and combining the laser welding technology, the innovation provides a larger process selection range for the welding, and the welding wire has remarkable significance and profound application prospects in the welding field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of steel material processing, and in particular to a welding material and a welding method for welding alloy steel. Background Art

[0002] Energy saving, emission reduction and consumption reduction have become important goals of the automotive industry, and lightweighting of the vehicle body is an important technical means of energy saving and consumption reduction. In order to reduce the thickness of the vehicle body material, ultra-high strength steel (steel with a tensile strength of ≥780MPa) is widely used in the vehicle body. In order to enhance corrosion resistance, anti-corrosion materials are generally coated on the surface of ultra-high strength steel, and then the plates containing ultra-high strength steel are combined to form the vehicle body or part of the vehicle body.

[0003] In the early technology, the body or body parts are generally formed by stamping, such as the hot stamping process disclosed in CN106466697A. However, this has high requirements for the stamping process, especially the stamping of ultra-high strength steel has many difficulties.

[0004] Using welding wire to weld the frame is an alternative solution, and resistance spot welding is a commonly used welding method. For ultra-high strength steel with coating, resistance spot welding will cause liquid metal embrittlement (LME). After the coating metal melts, it penetrates along the grain boundary of the steel plate substrate, causing the grain boundary bonding strength to decrease and cracking to occur easily.

[0005] CN116748676A discloses a method for laser welding alloy steel with aluminum-silicon coating on the surface. The welding strength is high, but this method has pores and sand holes, and the welding product yield is low. In addition, in this method, the nickel content in the welding wire must be strictly calculated according to the thickness, otherwise, the welding wire will form stainless steel during the laser sintering process and cannot be welded with ultra-high strength steel. Therefore, it is still necessary to find new welding methods and welding materials. Summary of the invention

[0006] The present application provides a welding material and a welding method for welding alloy steel to solve at least one problem raised in the above technical background.

[0007] To achieve the above objectives, this application adopts the following technical solutions:

[0008] The first aspect of the present application is to provide a welding material for welding alloy steel, wherein the alloy steel is an ultra-high strength steel with an anti-corrosion material coated on the surface, and the elements of the welding material include C, Si, Mn, Cr, Mo, Ni, and Fe, wherein the weight percentage of the elements is: C 0.08-0.15% based on the total weight of the welding material;

[0009] Si 0.30-0.65%;

[0010] Mn 0.90-2.20%;

[0011] Cr 25.0-28.0%;

[0012] Mo 0.07-0.13%;

[0013] Ni 19.0-24.3%;

[0014] The rest is Fe and inevitable impurities.

[0015] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of C is 0.09-0.12%, preferably 0.09-0.10%.

[0016] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Si is 0.40-0.55%, preferably 0.45-0.55%.

[0017] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Mn is 1.00-2.10%, preferably 1.80-2.05%.

[0018] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Mo is 0.10-0.12%, preferably 0.11-0.12%.

[0019] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Ni is 19.5-24.3%, preferably 20.0-24.3%.

[0020] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Cr is 25.5-28.0%, preferably 26.0-28.0%.

[0021] In a preferred embodiment, the welding material is in the form of powder, welding rod, or welding wire, and is particularly preferably in the form of welding wire.

[0022] In a preferred embodiment, the diameter of the welding wire is preferably 0.5-2 mm, preferably 1-1.5 mm, and more preferably 1.2-1.3 mm.

[0023] In a preferred embodiment, the anti-corrosion material is a metal coating, preferably at least one of zinc, nickel, chromium, aluminum, and aluminum silicon.

[0024] In a preferred embodiment, the elements of the alloy steel include: C, Si, Mn, P, S, Al, Ti, B, Cr, and Fe.

[0025] In a preferred embodiment, the composition weight percentage of the alloy steel is:

[0026] C 0.08-0.8%;

[0027] Si 0.05-1.0%;

[0028] Mn 0.1-5%;

[0029] P < 0.3%;

[0030] S<0.1%;

[0031] Al<0.3%;

[0032] Ti<0.5%;

[0033] B 0.0005-0.1%;

[0034] Cr 0.01-3%;

[0035] The rest is Fe and unavoidable impurities.

[0036] The second aspect of the present application is to provide a method for processing an alloy steel material, preferably a method for welding an alloy steel material, especially a method for welding ultra-high strength steel. Alternatively, the second aspect of the present application provides an application of the welding material, especially an application in welding ultra-high strength steel. Preferably, the ultra-high strength steel is an ultra-high strength steel with an anti-corrosion material coated on the surface, more preferably an ultra-high strength steel with a metal protective layer coated on the surface.

[0037] The processing method of the alloy steel or the application of the welding material described in the second aspect of the present application comprises the following steps:

[0038] Provide two workpieces to be welded and welding materials, wherein the workpieces to be welded are made of alloy steel, and the alloy steel is ultra-high strength steel with an anti-corrosion material coated on the surface;

[0039] Butt the welding areas of two workpieces to be welded, place welding material between the welding areas of the two workpieces to be welded, and melt the welding material by laser wire welding, so that the molten welding material covers at least a part of the welding area;

[0040] The molten welding material cools and solidifies, so that the two workpieces to be welded are connected into one.

[0041] In a preferred embodiment, the workpieces to be welded do not require pretreatment.

[0042] In a preferred embodiment, the laser wire welding melts the welding material through a laser spot.

[0043] Preferably, the diameter of the laser spot is larger than the diameter of the welding material.

[0044] In a preferred embodiment, based on the total weight of the welding material, the elements of the welding material include C, Si, Mn, Cr, Mo, Ni, and Fe.

[0045] Wherein, the weight percentage of the elements is:

[0046] C 0.08-0.15%;

[0047] Si 0.30-0.65%;

[0048] Mn 0.90-2.20%;

[0049] Cr 25.0-28.0%;

[0050] Mo 0.07-0.13%;

[0051] Ni 19.0-24.3%;

[0052] The rest is Fe and inevitable impurities.

[0053] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of C is 0.09-0.12%, preferably 0.09-0.10%.

[0054] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Si is 0.40-0.55%, preferably 0.45-0.55%.

[0055] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Mn is 1.00-2.10%, preferably 1.80-2.05%.

[0056] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Mo is 0.10-0.12%, preferably 0.11-0.12%.

[0057] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Ni is 19.5-24.3%, preferably 20.0-24.3%.

[0058] In a preferred embodiment, based on the total weight of the welding material, the weight percentage of Cr is 25.5-28.0%, preferably 26.0-28.0%.

[0059] In a preferred embodiment, the welding material is in the form of powder, welding rod, or welding wire, and is particularly preferably in the form of welding wire.

[0060] In a preferred embodiment, the diameter of the welding wire is preferably 0.5-2 mm, preferably 1-1.5 mm, and more preferably 1.2-1.3 mm.

[0061] In a preferred embodiment, the anti-corrosion material coated on the surface may be a metal coating, preferably at least one of zinc, nickel, chromium, aluminum, and aluminum silicon.

[0062] Preferably, the thickness of the metal coating plated on the surface is 10-100 μm, preferably 15-90 μm, and more preferably 20-80 μm.

[0063] In a preferred embodiment, the diameter of the welding wire is preferably 0.5-2 mm, preferably 1-1.5 mm, and more preferably 1.2-1.3 mm.

[0064] In a preferred embodiment, the elements of the alloy steel include: C, Si, Mn, P, S, Al, Ti, B, Cr, and Fe.

[0065] In a preferred embodiment, the composition weight percentage of the alloy steel is:

[0066] C 0.08-0.8%;

[0067] Si 0.05-1.0%;

[0068] Mn 0.1-5%;

[0069] P < 0.3%;

[0070] S<0.1%;

[0071] Al<0.3%;

[0072] Ti<0.5%;

[0073] B 0.0005-0.1%;

[0074] Cr 0.01-3%;

[0075] The rest is Fe and unavoidable impurities.

[0076] In a preferred embodiment, the thickness of the alloy steel to be welded is 0.5-5 mm, preferably 0.8-4 mm, and more preferably 1-3 mm.

[0077] In a preferred embodiment, in the laser wire welding, the laser power is 2-10 kW, preferably 2.5-8 kW, and more preferably 3-6 kW.

[0078] In a preferred embodiment, in the laser wire welding, the moving speed of the laser is 1-8 m / min, preferably 2-6 m / min, and more preferably 2-5 m / min.

[0079] In a preferred embodiment, in the laser wire welding, the wire feeding rate is 0.3-4 m / min, preferably 0.5-3 m / min, and more preferably 0.5-2 m / min.

[0080] In a preferred embodiment, the processing method of the alloy steel material to be welded may further include post-weld heat treatment.

[0081] Preferably, the post-weld heat treatment step comprises:

[0082] The alloy steel to be welded is heated to 880-950°C.

[0083] The heated alloy steel is subjected to stamping and then pressure-maintaining cooling and quenching.

[0084] Compared with the prior art, the technical solution of the present application has the following beneficial effects:

[0085] (1) The present application achieves a good welding effect by regulating the composition of the welding material. Compared with the alloy steel before welding, the material after welding using the welding material of the present application can still maintain a high mechanical strength and regularity. Its tensile strength can be as high as 1546MPa, which is equivalent to the alloy steel before welding, and its regular plastic extension strength Rp0.2 is as high as 1109MPa.

[0086] (2) The welding method of the present application is not just a simple connection of two parts, it actually forms a new, integrated structure between the materials. This integrated structure is more uniform and consistent in mechanical strength, and the weld and the parent material are well matched in performance, which improves the quality of the weld. The overall performance and stability of the material structure after welding are higher.

[0087] (3) Compared with the prior art such as CN116748676A, the welding materials and welding methods provided by the present application are used for welding ultra-high strength steel with anti-corrosion materials on the surface, which can reduce the sensitivity to the coating and have the advantage of reducing pores and cracking in the welding of various types of plates such as galvanized, nickel-plated, chrome-plated, and aluminum-silicon coated. Surprisingly, the laser welding of stainless steel welding wire with a specific elemental composition used in the present application has a higher yield of up to 99.99%. In addition, the present application realizes the welding of dissimilar steels between stainless steel welding wire and hot stamped steel plates by regulating the elemental composition and proportion of the welding wire and combining laser welding technology. This innovation provides a larger range of process options for this type of welding and has significant significance and far-reaching application prospects in the field of welding. BRIEF DESCRIPTION OF THE DRAWINGS

[0088] Figure 1 Photographs of the welded samples for this application;

[0089] Figure 2 This is a photo of the welded sample after tensile fracture for this application;

[0090] Figure 3 The photos for this application are cut and spliced ​​along the fracture surface;

[0091] Figure 4 The weld size and matrix microstructure photos of welding sample 1 for this application;

[0092] Figure 5 The weld size and matrix microstructure photos of welding sample 2 for this application;

[0093] Figure 6 The weld size and matrix microstructure photos of welding sample 3 for this application;

[0094] Figure 7 Photos of weld size and matrix microstructure of welding sample 4 for this application. DETAILED DESCRIPTION

[0095] The present application provides a welding method and welding material for ultra-high strength steel with metal coating on the surface. In order to make the purpose, technical solution and effect of the present application clearer and more specific, the present application is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the content of the present application and are not used to limit the content of the present application.

[0096] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0097] Embodiment 1:

[0098] This embodiment provides a welding method for ultra-high strength steel, which is a kind of steel with extremely high strength, greater than 1000 MPa, and is widely used in aerospace, automobile, construction, bridge and other fields:

[0099] Select the plate to be welded with aluminum silicon coating on the surface, and cut the plate into dumbbell-shaped specimens with the size of 240mm long × 20mm wide × 1.2mm thick, such as Figure 1 As shown. The weight percentage of the components of the plate is: C 0.8%, Si 1.0%, Mn2%, P<0.3%, S<0.1%, Al<0.3%, Ti<0.5%, B 0.1%, Cr 0.5%, and the rest is Fe and unavoidable impurities. The average thickness of the aluminum-silicon coating on the upper and lower surfaces of the plate is 5μm and 5μm respectively;

[0100] The dumbbell-shaped specimens were randomly cut and then laser wire welding was performed on the fracture surface. Figure 1 As shown, the welding power is 5950W, the moving speed of the laser is 5m / min, the selected solder is solid welding wire, and the brand of welding wire is CmC M118Cr series (Shanghai Xingang Technology Co., Ltd.);

[0101] Among them, according to weight percentage, the weight percentage of Ni element in the welding wire is 24.3%, the weight percentage of Cr element is 28%, the weight percentage of other elements is C: 0.1%, Mn: 2.0%, Si: 0.5%, Mo: 0.35%, and the rest is iron and unavoidable impurities. The diameter of the welding wire is 1.0 mm, and the wire feeding speed is 3.0 m / min;

[0102] The welded specimen was heat treated at 950°C for 5 minutes, and then quickly transferred to a mold with cooling water circulating inside for compaction (pressure cooling for 15 seconds, the nominal force of the press was 1000KN, and the cooling rate was greater than 30°C / s), to obtain welding sample 1;

[0103] The processed welding sample 1 was subjected to tensile test and metallographic inspection and analysis.

[0104] Embodiment 2:

[0105] This embodiment provides a welding method for ultra-high strength steel, which is a kind of steel with extremely high strength, greater than 1000 MPa, and is widely used in aerospace, automobile, construction, bridge and other fields:

[0106] Select the plate to be welded with aluminum silicon coating on the surface, cut the plate into dumbbell-shaped specimens with the size of 240mm long×20mm wide×1.2mm thick, the composition weight percentage of the plate is: C 0.8%, Si1.0%, Mn 2%, P<0.3%, S<0.1%, Al<0.3%, Ti<0.5%, B 0.1%, Cr 0.5%, the rest is Fe and unavoidable impurities. The average thickness of the aluminum silicon coating on the upper and lower surfaces of the plate is 5μm and 5μm respectively;

[0107] The dumbbell-shaped specimens were randomly cut, and then the fracture surfaces were subjected to laser wire welding. The welding power was 4800 W, the laser moving speed was 4.5 m / min, and the selected solder was solid welding wire, the grade of which was CmC M118Cr series (Shanghai Xingang Technology Co., Ltd.);

[0108] According to weight percentage, the weight percentage of Ni element in the welding wire is 23.8%, the weight percentage of Cr element is 27%, the weight percentage of other elements is C: 0.1%, Mn: 2.0%, Si: 0.5%, Mo: 0.35%, and the rest is iron and unavoidable impurities. The diameter of the welding wire is 1.0 mm, and the wire feeding speed is 2.8 m / min;

[0109] The welded specimens were heat treated at a temperature of 950°C for 5 minutes, and then quickly transferred to a mold with cooling water circulating inside for compaction (pressure cooling for 15 seconds, the nominal force of the press was 1000KN, and the cooling rate was greater than 30°C / s), to obtain welded sample 2;

[0110] The processed welding sample 2 was subjected to tensile test and metallographic inspection and analysis.

[0111] Embodiment 3:

[0112] This embodiment provides a welding method for ultra-high strength steel, which is a kind of steel with extremely high strength, greater than 1000 MPa, and is widely used in aerospace, automobile, construction, bridge and other fields:

[0113] Select the plate to be welded with aluminum silicon coating on the surface, cut the plate into dumbbell-shaped specimens with the size of 240mm long×20mm wide×1.2mm thick, the composition weight percentage of the plate is: C 0.8%, Si1.0%, Mn 2%, P<0.3%, S<0.1%, Al<0.3%, Ti<0.5%, B 0.1%, Cr 0.5%, the rest is Fe and unavoidable impurities. The average thickness of the aluminum silicon coating on the upper and lower surfaces of the plate is 5μm and 5μm respectively;

[0114] The dumbbell-shaped specimens were randomly cut, and then the fracture surfaces were subjected to laser wire welding. The welding power was 3850 W, the laser moving speed was 3.5 m / min, and the selected solder was solid welding wire, the grade of which was CmC M118Cr series (Shanghai Xingang Technology Co., Ltd.);

[0115] According to weight percentage, the weight percentage of Ni element in the welding wire is 22.3%, the weight percentage of Cr element is 25%, the weight percentage of other elements is C: 0.1%, Mn: 2.0%, Si: 0.5%, Mo: 0.35%, and the rest is iron and unavoidable impurities. The diameter of the welding wire is 1.0 mm, and the wire feeding speed is 2.5 m / min;

[0116] The welded specimens were heat treated at a temperature of 950°C for 5 minutes, and then quickly transferred to a mold with cooling water circulating inside for compaction (pressure cooling for 15 seconds, the nominal force of the press was 1000KN, and the cooling rate was greater than 30°C / s), to obtain welded sample 3;

[0117] The processed welding sample 3 was subjected to tensile test and metallographic inspection and analysis.

[0118] Embodiment 4:

[0119] This embodiment provides a welding method for ultra-high strength steel, which is a kind of steel with extremely high strength, greater than 1000 MPa, and is widely used in aerospace, automobile, construction, bridge and other fields:

[0120] Select the plate to be welded with aluminum silicon coating on the surface, cut the plate into dumbbell-shaped specimens with the size of 240mm long×20mm wide×1.2mm thick, the composition weight percentage of the plate is: C 0.8%, Si1.0%, Mn 2%, P<0.3%, S<0.1%, Al<0.3%, Ti<0.5%, B 0.1%, Cr 0.5%, the rest is Fe and unavoidable impurities. The average thickness of the aluminum silicon coating on the upper and lower surfaces of the plate is 5μm and 5μm respectively;

[0121] The dumbbell-shaped specimens were randomly cut, and then the fracture surfaces were subjected to laser wire welding. The welding power was 3500 W, the laser moving speed was 3.0 m / min, and the selected solder was solid welding wire, the grade of which was CmC M118Cr series (Shanghai Xingang Technology Co., Ltd.);

[0122] According to weight percentage, the weight percentage of Ni element in the welding wire is 20.0%, the weight percentage of Cr element is 26%, the weight percentage of other elements is C: 0.1%, Mn: 2.0%, Si: 0.5%, Mo: 0.35%, and the rest is iron and unavoidable impurities. The diameter of the welding wire is 1.0 mm, and the wire feeding speed is 1.8 m / min;

[0123] The welded specimens were heat treated at a temperature of 950°C for 5 minutes, and then quickly transferred to a mold with cooling water circulating inside for compaction (pressure cooling for 15 seconds, the nominal force of the press was 1000KN, and the cooling rate was greater than 30°C / s), to obtain welded sample 4;

[0124] The processed welding sample 4 was subjected to tensile test and metallographic inspection and analysis.

[0125] Comparative Example 1:

[0126] This comparative example provides a resistance welding method:

[0127] The same plate as in Example 1 was used to cut dumbbell-shaped specimens of the same size. The dumbbell-shaped specimens were randomly cut and then welded on the fractured surfaces. The material of the welding wire was also the same as in Example 1.

[0128] The welding sample obtained by resistance welding in this comparative example showed obvious cracking, and after the weld was cut open, many sand holes and pores were found.

[0129] Comparative Example 2:

[0130] This comparative example provides an arc welding method:

[0131] The same plate as in Example 1 was used to cut dumbbell-shaped specimens of the same size. The dumbbell-shaped specimens were randomly cut and then welded on the fractured surfaces. The material of the welding wire was also the same as in Example 1.

[0132] The welding samples obtained by arc welding in this comparative example have the phenomenon of non-smooth transition with the base material, poor welding joints, and uneven welds. After cutting the welds, many sand holes and pores are found.

[0133] The tensile test results of the steel plate welded parts of Examples 1-4 are shown in Table 1, wherein the tensile test method refers to GB / T228.1-2021, the testing equipment uses a WEW-300 microcomputer-controlled universal testing machine, a ZES-(25-10) electronic extensometer, and a 0-200 digital caliper, the sample thickness is 1.2 mm, the dumbbell-shaped specimen, the parallel part width is 12.4 mm, the original gauge length is 20 mm, and the photos before and after the inspection are as follows: Figure 1 , 2 shown.

[0134] Table 1, tensile test results of steel plate welding samples of Examples 1-4 of the present application

[0135]

[0136] According to Table 1, it can be seen that the content of Ni and Cr in the welding wire is relatively high, and the welding effect is good. The material after welding in this application still has a relatively high mechanical strength. The fracture positions of Examples 2-4 are all located on the parent material, which shows that the welding of this application is not just a simple connection of two parts together. It actually forms a new, integrated structure between the materials. This integrated structure is more uniform and consistent in mechanical strength, and can therefore withstand greater forces. Although the fracture position of Example 1 is located at the weld, its tensile strength is as high as 1542MPa, which is consistent with the tensile strength of the parent material. It can be seen that the weld and the parent material have achieved a good match in performance, and the welded joint has high quality. In addition, the regular plastic extension strength Rp0.2 of the material after welding in this application is as high as 1109MPa, and the material has a high regularity, which means that there are no obvious defects or flaws in the welding process of this application, and the weld quality is good, ensuring the overall performance and stability of the welded structure, and achieving excellent welding technology and precise control capabilities.

[0137] The metallographic inspection and analysis method of the welded steel plate in this application refers to GB / T 15125-2009, and the inspection equipment includes AOSVI's M330-HD228S metallographic microscope, Iqiege-180D (formerly SQ80) electronic component cutting machine, MP-2 metallographic sample grinding and polishing machine, and XQ-2B metallographic mounting machine;

[0138] The test results are as follows:

[0139] Example 1 The weld size of the welded sample is as follows Figure 4 As shown, there are no pores or crack defects on the cross section of the sample weld, and the weld shape is in good condition according to the metallographic inspection and analysis of the weld.

[0140] The weld size of the welding sample of Example 2 is as follows Figure 5 As shown, there are no pores or cracks on the cross section of the sample weld. The weld size is shown in Figure 2 , the regularity of the weld shape is better.

[0141] The weld size of the welding sample of Example 3 is as follows Figure 6 As shown, there are no pores or cracks on the cross section of the weld of the sample, and the weld size is Figure 3 .

[0142] Example 4 The weld size of the welded sample is as follows Figure 7 As shown in the figure, there are no pores or cracks on the cross section of the weld of the sample, and the weld size is Figure 4 It can be found that the regularity of the weld shape is good and the uniformity of the weld molten structure is good.

[0143] According to the results of metallographic inspection and analysis, it can be seen that the welding method and welding materials provided in this application can reduce the sensitivity to the plate coating, and have the advantage of reducing pores, sand holes and cracking in the welding of various types of plates such as galvanized, nickel-plated, chromium-plated, and aluminum-silicon-plated.

[0144] The present application is not limited to the welding of aluminum-silicon plate materials, but can also be used for welding various types of plates such as galvanized, nickel-plated, and chrome-plated, and can achieve the above-mentioned welding effect, thereby meeting the needs of different fields.

[0145] Compared with CN116748676A, the welding method and welding materials provided by this application are used for welding ultra-high strength steel plates with anti-corrosion materials on the surface, with a higher yield rate of up to 99.99%. In addition, this application realizes the welding of dissimilar steels of stainless steel welding wire and hot stamping steel plates by adjusting the element composition and proportion of the welding wire and combining laser welding technology. This innovation provides a wider range of process options for such welding, which has significant significance and far-reaching application prospects in the field of welding.

[0146] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.

Claims

1. A welding material for welding alloy steel, characterized in that: The alloy steel is an ultra-high strength steel with an anti-corrosion material coated on the surface. The elements of the welding material include C, Si, Mn, Cr, Mo, Ni, and Fe. Based on the total weight of the welding material, Wherein, the weight percentage of the elements is: C 0.08-0.15%; Si 0.30-0.65%; Mn 0.90-2.20%; Cr 25.0-28.0%; Mo 0.07-0.13%; Ni 19.0-24.3%; The rest is Fe and inevitable impurities.

2. The welding material according to claim 1, characterized in that: The welding material may be in the form of powder, welding rod, or welding wire, and welding wire is particularly preferred.

3. The welding material according to claim 2, characterized in that: The diameter of the welding wire is 0.5-2 mm, preferably 1-1.5 mm, and more preferably 1.2-1.3 mm.

4. The welding material according to claim 1, characterized in that: The anti-corrosion material is a metal coating, preferably at least one of zinc, nickel, chromium, aluminum, and aluminum silicon coatings.

5. The welding material according to claim 1, characterized in that: The elements of the alloy steel include: C, Si, Mn, P, S, Al, Ti, B, Cr, Fe; Wherein, the weight percentage of the elements is: C 0.08-0.8%; Si 0.05-1.0%; Mn 0.1-5%; P<0.3%; S<0.1%; Al<0.3%; Ti<0.5%; B 0.0005-0.1%; Cr 0.01-3%; The rest is Fe and unavoidable impurities.

6. A welding method, characterized in that: The following steps are involved: Provide two workpieces to be welded and the welding material according to any one of claims 1 to 5, wherein the material of the workpieces to be welded is alloy steel, and the alloy steel is ultra-high strength steel with an anti-corrosion material coated on the surface; Butt the welding areas of two workpieces to be welded, place welding material between the welding areas of the two workpieces to be welded, and melt the welding material by laser wire welding, so that the molten welding material covers at least a part of the welding area; The molten welding material cools and solidifies, so that the two workpieces to be welded are connected into one.

7. The welding method according to claim 6, characterized in that: In the laser wire welding step, the laser power is 2-10 kW, preferably 2.5-8 kW, more preferably 3-6 kW; and / or The moving speed of the laser is 1-8 m / min, preferably 2-6 m / min, more preferably 2-5 m / min; and / or The wire feeding rate is 0.3-4 m / min, preferably 0.5-3 m / min, and more preferably 0.5-2 m / min.

8. The welding method according to claim 6, characterized in that: The welding method further comprises a post-weld heat treatment step; Preferably, the post-weld heat treatment step comprises: Heat the connected workpieces to 880-950℃. The heated workpiece is stamped and then cooled and quenched under pressure.