Galvanizing method for steel pipe tower steel member
By using a shot blasting machine to remove rust and roughen the galvanizing technology of steel pipe tower steel components, and adjust the structure of the shot blasting device, the problem of zinc layer thickness and uniformity is solved, and the galvanizing thickness and adhesion is improved. , suitable for steel plate treatment of different widths.
Patent Information
- Application Number
- CN202410932165.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing steel pipe tower steel components galvanizing technology, the thickness of the zinc layer of the steel plate is difficult to meet the requirements, and the width of the discharge port of the shot blasting machine is inconvenient to adjust, resulting in uneven zinc layer and affecting the galvanizing effect.
Before unloading the steel plate, use a shot blasting machine to remove rust and roughen it. By adjusting the inner impeller and adjustment hole of the shot blaster, the tangential throwing and uniformity of the abrasive at the discharge port are ensured, and the width of the discharge port is adjusted. , suitable for steel plates of different widths, ensuring galvanized thickness and adhesion.
The steel pipe and the connecting plate are synchronized to meet the required thickness requirements during galvanization, the adhesion and galvanization efficiency of the zinc layer are improved, and a uniform roughened surface of the steel plate is obtained, which is suitable for steel plate treatment of different widths.
Smart Images

Figure CN118905558A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel tube tower preparation, in particular to a galvanizing method for steel components of a steel tube tower. Background Art
[0002] Since the steel components of the steel pipe tower are mainly pipes and connecting plates welded together, the thickness of the pipe is usually thinner and the thickness of the steel plate is thicker. Since the thickness of the galvanized layer is determined by the thickness of the material, the minimum thickness of the zinc layer is often determined by the thickness of the material. The zinc layer thickness of the pipe has reached the requirement, but the thickness of the connecting plate welded together does not meet the requirement.
[0003] In addition, the width of the discharge port of the existing shot blasting machine is usually fixed, which is not convenient to adjust according to the width of the steel plate. Moreover, the abrasive at the discharge port is mostly discharged in a disorderly manner. After being thrown out at high speed by the impeller, it is easy to cause uneven coarsening of the steel plate surface. Summary of the invention
[0004] The invention provides a galvanizing method for steel components of a steel pipe tower. Before the steel plates are cut, a shot blasting machine is used to remove rust and roughen the surfaces of the steel plates, so that the steel pipes and connecting plates can simultaneously reach the required thickness requirements during galvanizing.
[0005] The technical solution of the present invention is achieved in this way: a galvanizing method for a steel pipe tower steel component comprises the following steps:
[0006] (1) Using a shot blasting machine to remove rust and roughen the surface of the steel plate, and then cutting the steel plate to prepare a continuous plate;
[0007] (2) making holes in the connecting plate, bending it, and then welding it with the steel pipe to obtain a steel component;
[0008] (3) The steel components are galvanized.
[0009] Furthermore, in step (1), the parameters of shot blasting and rust removal are: the spraying angle is 60-75°, and the spraying distance is 100-300 mm.
[0010] Furthermore, in step (3), during the galvanizing process, the steel component is continuously shaken to change the position of each contact point of the steel component; after the steel component is dipped, it is lifted at 2 m / min, and the angle of the steel component is adjusted during the lifting process until the steel component is completely exposed to the zinc liquid, and then lifted at 8 m / min until the steel component is completely out of the zinc pot, and then the remaining zinc is shaken off and cooled.
[0011] Furthermore, in step (3), if the thickness of the steel component is ≥5 mm, the minimum thickness of the galvanized steel component is 85 μm, and the average thickness is 100 μm; if the thickness of the steel component is <5 mm, the minimum thickness of the galvanized steel component is 65 μm, and the average thickness is 75 μm.
[0012] Further, in step (3), the steel component is Q235 steel, the thickness of the steel component is ≤4mm, the galvanizing temperature is 439-443℃, and the time is 140s; the thickness of the steel component is 5-8mm, the galvanizing temperature is 439-443℃, and the time is 150s; the thickness of the steel component is 10-14mm, the galvanizing temperature is 438-442℃, and the time is 160s; the thickness of the steel component is ≥16mm, the galvanizing temperature is 437-441℃, the thickness of the steel component is 16-24mm, the galvanizing time is 180s, the thickness of the steel component is ≥25mm, and the galvanizing time is 200s; the end temperature of galvanizing is 2±2℃ lower than the initial temperature.
[0013] Furthermore, in step (3), the steel component is Q345 steel, Q355 steel or Q420 steel, the thickness of the steel component is ≤8 mm, the galvanizing temperature is 439-442°C, and the time is 140 s; the thickness of the steel component is 10-14 mm, the galvanizing temperature is 438-441°C, and the time is 150 s; the thickness of the steel component is ≥16 mm, the galvanizing temperature is 437-441°C, the thickness of the steel component is 16-18 mm, the galvanizing time is 180 s, the thickness of the steel component is 20-24 mm, the galvanizing time is 190 s, the thickness of the steel component is ≥25 mm, and the galvanizing time is 200 s; the end temperature of galvanizing is 2±2°C lower than the initial temperature.
[0014] Further, in step (1), the shot blasting machine includes a shot blasting chamber, a shot blasting device is arranged in the shot blasting chamber, the shot blasting device includes an outer shell, a rotating inner impeller is arranged in the outer shell, a rotating outer impeller is arranged on the outer side of the inner impeller, a fixing sleeve is arranged between the outer impeller and the inner impeller, the fixing sleeve is fixedly connected to the outer shell, a discharge port is arranged on the fixing sleeve, a spacing ring is slidably inserted on the inner impeller, an adjusting tube is rotatably connected to the inner side of the spacing ring, the adjusting tube and the spacing ring slide axially synchronously, an adjusting hole is arranged on the adjusting tube, the adjusting hole is located on the left side of the spacing ring, the adjusting hole and the discharge port are circumferentially staggered, the left end of the adjusting tube is slidably placed in a temporary storage tank, and the upper end of the temporary storage tank is connected to the feeding tube.
[0015] Furthermore, the inner diameter of the temporary storage tank is larger than that of the feeding tank, and a baffle plate is provided in the feeding pipe. The right end of the baffle plate is hinged to the inner wall of the feeding pipe, and the left end is a free end. The left end of the adjusting tube is against the lower side of the baffle plate, and the left end of the adjusting tube is an inclined surface inclined downward, and a feed port is provided.
[0016] Furthermore, the inner impeller and the outer impeller are both connected to the right end plate, and the right end plate is driven to rotate by the shot blasting motor.
[0017] Beneficial effects of the present invention:
[0018] The present invention adds a shot blasting machine to remove rust and roughen the surface of the steel plate before the steel plate is cut. On the one hand, rust is deeply removed, and on the other hand, a uniform roughened surface is obtained, which is beneficial to increase the galvanizing thickness and the adhesion of the zinc layer, thereby allowing the steel pipe and the connecting plate to simultaneously reach the required thickness requirements during galvanizing.
[0019] The shot blasting machine of the present invention increases the inner impeller and cooperates with the adjusting hole of the adjusting tube, so that the abrasive at the discharge port is thrown out tangentially and then thrown out at high speed by the outer impeller, which is beneficial to obtaining a uniform roughened surface of the steel plate and improving the shot blasting efficiency at the same time; the discharge width of the discharge port is adjusted by the axial movement of the spacer ring and the adjusting tube, which is suitable for shot blasting of steel plates of different widths, and the setting of the spacer ring does not affect the rotation of the inner impeller; when the adjusting tube moves axially, the left end of the material baffle plate can be synchronously pushed up and down to swing, thereby adjusting the feeding amount of the abrasive. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 It is a structural schematic diagram of the shot blasting machine;
[0022] Figure 2 It is the left view of the inner and outer impellers.
[0023] Outer shell 1, inner impeller 2, outer impeller 3, right end plate 4, shot blasting motor 5, fixing sleeve 6, spacer ring 7, adjusting tube 8, linear drive module 9, adjusting hole 10, baffle plate 11, feeding tube 12, feeding port 13, discharging port 14, temporary storage tank 15. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] A galvanizing method for a steel pipe tower steel component comprises the following steps:
[0027] (1) Use a shot blasting machine to remove rust and roughen the surface of the steel plate until the metal surface presents a grayish white metal appearance and a uniform roughened surface. The surface rust removal level should reach Sa2.5 level required by GB8923.1, and the surface roughness should reach RZ40μm-80μm (Ra 12.5μm-20μm);
[0028] Parameters of shot blasting and rust removal: the spray angle is 60-75°, the spray distance is 100-300mm, and then the steel plate is cut to prepare the continuous plate;
[0029] (2) Making holes in the connecting plate, bending it, and then welding it to the steel pipe to obtain the steel components required for the steel pipe tower;
[0030] (3) The steel components are galvanized in the following order: black parts inspection, loading and unloading, pickling, rinsing, plating agent treatment, secondary loading, preheating and drying, hot dip galvanizing, water cooling, passivation, unloading, inspection, correction, and storage.
[0031] Pickling: The concentration of the newly prepared acid solution should reach 18-25%. When the concentration drops to 4% and the iron content is 120 g / L, and it affects the production progress, it should be replaced and the acid pool should be cleaned after replacement.
[0032] Water cooling: The cooling water temperature must be maintained between 25-60℃, the water quality must be clear, the water flow must be constant, and the PH value must be 6-8.
[0033] Passivation: The passivation liquid is prepared with chromium-free passivating agent and clean water in a ratio of 1:20. The working temperature is natural room temperature and the PH is 1.5-2.0.
[0034] Hot-dip galvanizing: The zinc liquid level should be 100-150mm away from the zinc pot surface (to prevent zinc liquid from overflowing when the parts are plated); when the zinc slag thickness exceeds 100mm, the slag should be removed immediately. During the dipping process, the position of each contact point of the steel component should be changed by slowly lifting and lowering (shaking) a little bit (especially for plated pipes) to avoid leakage caused by poor exhaust.
[0035] After the steel components are impregnated, the rack is slowly lifted at 2 meters per minute, and the rack angle is adjusted during the process until the steel components are completely exposed to the zinc liquid. Then, it is quickly lifted at 8 meters per minute. After all the steel components leave the zinc pot, the rack is quickly shaken with an iron hook (to shake off the remaining zinc) and then quickly sent to the cooling tank for cooling to avoid color difference caused by long-term air cooling.
[0036] Angle control when galvanizing steel components:
[0037] Component Type Angle of entering zinc pool Zinc pool exit angle Main material of steel components 50±5° 40±5° Steel component auxiliary materials 85±5° 80±5°
[0038] Galvanizing temperature and time of steel components:
[0039]
[0040] The minimum thickness of the galvanized layer of steel components is shown in the following table:
[0041] Parts and their thickness / mm Minimum thickness / μm Average thickness / μm Steel parts, ≥5 85 100 Steel parts, <5 65 75
[0042] Example 2
[0043] This embodiment is basically the same as the embodiment 1, except that the shot blasting machine includes a shot blasting chamber, and a shot blasting device is arranged in the shot blasting chamber, such as Figure 1 and 2 As shown, the shot blasting machine includes an outer shell 1, a rotating inner impeller 2 is arranged in the outer shell 1, and a rotating outer impeller 3 is spaced apart on the outer side of the inner impeller 2. The inner impeller 2 and the outer impeller 3 are both connected to the right end plate 4, and the right end plate 4 is rotatably connected to the outer shell 1 through a bearing and is driven to rotate by a shot blasting motor 5.
[0044] A fixed sleeve 6 is provided between the outer impeller 3 and the inner impeller 2. The left end of the fixed sleeve 6 is fixedly connected to the outer shell 1, and the right end is a free end. A discharge port 14 is axially provided on the side wall of the fixed sleeve 6. A spacer ring 7 is slidably inserted on the inner impeller 2. An adjusting tube 8 is rotatably connected to the inner side of the spacer ring 7. The adjusting tube 8 and the spacer ring 7 slide axially synchronously, and the spacer ring 7 can rotate with the inner impeller 2. A linear drive module 9 is fixed on the outer side of the outer shell 1. The linear drive module 9 is connected to the adjusting tube 8, thereby driving the adjusting tube 8 and the spacer ring 7 to slide axially. The linear drive module 9 can be a ball screw driven by a motor, or other structures.
[0045] The adjusting tube 8 is provided with an adjusting hole 10, which is located on the left side of the spacing ring 7. The adjusting hole 10 and the discharge port 14 are circumferentially staggered. The left end of the adjusting tube 8 is slidably placed in the temporary storage tank 15, and the upper end of the temporary storage tank 15 is connected to the feeding tube 12. Through the setting of the spacing ring 7, the space between the fixed sleeve 6 and the adjusting tube 8 is divided into two parts, left and right. After the abrasive is discharged through the adjusting hole 10, it is driven by the rotating inner blades and thrown out tangentially from the discharge port 14 on the left side of the spacing plate. Through the axial movement of the adjusting tube 8 and the spacing ring 7, the length of the adjusting hole 10 in the housing 1 is adjusted, and then the width of the discharge is adjusted. It is suitable for shot blasting of steel plates of different widths, and the abrasive is thrown out tangentially in cooperation with the circumferentially rotating inner impeller 2, which is convenient for the outer impeller 3 to throw out at high speed and uniformly, and the surface of the steel plate is shot blasted, which is conducive to obtaining a uniform roughened surface and improving the shot blasting efficiency.
[0046] like Figure 1As shown, the inner diameter of the temporary storage tank 15 is larger than the feeding tube 12, and a baffle plate 11 is arranged in the feeding tube 12. The right end of the baffle plate 11 is hinged to the inner wall of the feeding tube 12, and the left end is a free end. The left end of the adjusting tube 8 is against the lower side of the baffle plate 11, and the left end of the adjusting tube 8 is an inclined surface inclined downward, and a feed port 13 is arranged. When the adjusting tube 8 moves axially left and right, the left end of the baffle plate 11 is pushed to swing up and down, thereby adjusting the feed amount of the abrasive. If the adjusting tube 8 moves left, the discharge width of the discharge port 14 becomes narrower, and at the same time, the left end of the adjusting tube 8 pushes the baffle plate 11 to swing upward, and the discharge port in the feeding tube 12 becomes narrower, and the feed amount is reduced.
[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for galvanizing a steel pipe tower steel component, characterized in that: The following steps are involved: (1) Using a shot blasting machine to remove rust and roughen the surface of the steel plate, and then cutting the steel plate to prepare a continuous plate; (2) making holes in the connecting plate, bending it, and then welding it with the steel pipe to obtain a steel component; (3) The steel components are galvanized.
2. The galvanizing method for a steel pipe tower steel member according to claim 1, characterized in that: In step (1), the parameters of shot blasting and rust removal are: the spraying angle is 60-75°, and the spraying distance is 100-300 mm.
3. The galvanizing method for a steel pipe tower steel member according to claim 1, characterized in that: In step (3), during the galvanizing process, the steel component is continuously shaken to change the position of each contact point of the steel component; after the steel component is dipped, it is lifted at 2 m / min, and the angle of the steel component is adjusted during the lifting process until the steel component is completely exposed to the zinc liquid, and then lifted at 8 m / min until the steel component is completely out of the zinc pot, and then the excess zinc is shaken off and cooled.
4. The galvanizing method for a steel pipe tower steel member according to claim 1, characterized in that: In step (3), if the thickness of the steel component is ≥5 mm, the minimum thickness of the galvanized steel component is 85 μm and the average thickness is 100 μm; if the thickness of the steel component is <5 mm, the minimum thickness of the galvanized steel component is 65 μm and the average thickness is 75 μm.
5. A galvanizing method for a steel pipe tower steel member according to claim 4, characterized in that: In step (3), the steel component is Q235 steel, the thickness of the steel component is ≤4mm, the galvanizing temperature is 439-443℃, and the time is 140s; the thickness of the steel component is 5-8mm, the galvanizing temperature is 439-443℃, and the time is 150s; the thickness of the steel component is 10-14mm, the galvanizing temperature is 438-442℃, and the time is 160s; the thickness of the steel component is ≥16mm, the galvanizing temperature is 437-441℃, the thickness of the steel component is 16-24mm, the galvanizing time is 180s, the thickness of the steel component is ≥25mm, and the galvanizing time is 200s; the end temperature of galvanizing is 2±2℃ lower than the initial temperature.
6. A galvanizing method for steel pipe tower steel components according to claim 4, characterized in that: In step (3), the steel component is Q345 steel, Q355 steel or Q420 steel, the thickness of the steel component is ≤8mm, the galvanizing temperature is 439-442°C, and the time is 140s; the thickness of the steel component is 10-14mm, the galvanizing temperature is 438-441°C, and the time is 150s; the thickness of the steel component is ≥16mm, the galvanizing temperature is 437-441°C, the thickness of the steel component is 16-18mm, the galvanizing time is 180s, the thickness of the steel component is 20-24mm, the galvanizing time is 190s, the thickness of the steel component is ≥25mm, and the galvanizing time is 200s; the end temperature of galvanizing is 2±2°C lower than the initial temperature.
7. The galvanizing method for a steel pipe tower steel member according to claim 1, characterized in that: In step (1), the shot blasting machine includes a shot blasting chamber, a shot blasting device is arranged in the shot blasting chamber, the shot blasting device includes an outer shell, a rotating inner impeller is arranged in the outer shell, a rotating outer impeller is arranged on the outer side of the inner impeller, a fixing sleeve is arranged between the outer impeller and the inner impeller, the fixing sleeve is fixedly connected to the outer shell, a discharge port is arranged on the fixing sleeve, a spacing ring is slidably inserted on the inner impeller, an adjusting tube is rotatably connected to the inner side of the spacing ring, the adjusting tube and the spacing ring slide axially synchronously, an adjusting hole is arranged on the adjusting tube, the adjusting hole is located on the left side of the spacing ring, the adjusting hole and the discharge port are circumferentially staggered, the left end of the adjusting tube is slidably placed in a temporary storage tank, and the upper end of the temporary storage tank is connected to the feeding tube.
8. A method for galvanizing a steel pipe tower steel member according to claim 7, characterized in that: The inner diameter of the temporary storage tank is larger than that of the feeding tank. A baffle plate is arranged in the feeding pipe. The right end of the baffle plate is hinged to the inner wall of the feeding pipe, and the left end is a free end. The left end of the adjusting pipe is against the lower side of the baffle plate. The left end of the adjusting pipe is an inclined surface inclined downward and is provided with a feed port.
9. A method for galvanizing a steel pipe tower steel member according to claim 8, characterized in that: The inner impeller and the outer impeller are both connected to the right end plate, and the right end plate is driven to rotate by the shot blasting motor.
Citation Information
Patent Citations
Zinc fingre anticorrosion steel pipe pole and preparation method thereof
CN109468063A
Hot galvanizing process for iron tower components and hot plating liquid system
CN110129703A
Steel plate uncoiling line shot blasting machine suitable for different widths
CN116551577A
Charging Apparatus for raw material and method thereof
KR1020210058666A