Preparation method of graphene powder
Through the improved Hummers method and high-temperature calcination steps, the precise control and macro-preparation problems in the preparation of oligolayer graphene materials are solved, and graphene powder with high conductivity and fast charging performance is achieved, satisfying the high energy density of lithium batteries and Fast charging demand.
Patent Information
- Application Number
- CN202411144618.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-20
AI Technical Summary
It is difficult to accurately control and macro-preparation of oligolayer graphene materials in the prior art, and the presence of dispersants in common methods will affect the high-voltage resistance and fast charging requirements of lithium-ion batteries.
Graphene oxide (GO) was prepared in batches by the improved Hummers method, reducing the concentration of GO in water, separated and dried after reduction with chemical reagents, followed by high-speed stirring in a closed container for fluffing, and finally calcined at high temperature to prepare oligos Graphene powder.
The macro preparation of graphene powder has been realized, the conductivity and application value have been improved, and the high energy density and fast charging performance support for lithium batteries.
Smart Images

Figure CN118908194A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of thin-layer graphene materials, and in particular to a method for preparing low-layer graphene. Background Art
[0002] Graphene is a carbon atom 2 The two-dimensional structure layer formed by hybridization is honeycomb-shaped and is the basic structural unit of other carbon materials. Since its advent, it has been a research hotspot in the field of materials science due to its outstanding physical and chemical properties.
[0003] Few-layer graphene generally refers to graphene with less than 5 layers. Compared with other multi-layer graphene, few-layer graphene is thinner and more flexible, and has outstanding performance in nanoelectronic devices, composite materials, etc. Adding few-layer graphene to batteries can increase conductivity, enhance battery capacity and cycle life.
[0004] There are many methods for preparing graphene, including mechanical exfoliation, liquid phase exfoliation, chemical oxidation, crystal epitaxial growth, chemical vapor deposition, organic synthesis and carbon nanotube exfoliation.
[0005] The mechanical exfoliation method is to overcome the interaction between the sheets in the graphite by mechanical means, separate the graphite using photoresist, and successfully obtain a single layer of graphene. Although this method can produce fewer graphene layers than the general mechanical exfoliation method, it is still difficult to accurately control the purity of graphene and the yield is extremely low, making it difficult to achieve large-scale preparation of graphene. The currently commercialized mechanical exfoliation method generally uses sand mills, homogenizers and other means to break and peel the graphite. The thickness of the obtained graphene material is generally ≥10 layers, which belongs to multi-layer graphene material. It is impossible to prepare graphene with few or few layers, and a small amount of dispersant needs to be added to stabilize the graphene while these devices are breaking and peeling. The dispersant will have adverse effects during the use of downstream lithium-ion batteries, and it is impossible to achieve higher-end applications of graphene materials.
[0006] The liquid phase exfoliation method uses ultrasound, heating and other means to exfoliate graphite to prepare single-layer or multi-layer graphene solutions. This method requires the addition of a lot of dispersants in the process of preparing graphene. The dispersant has the function of stabilizing the graphene sheets in the graphene solution. However, when preparing lithium-ion batteries downstream, the dispersant on the surface of graphene as a conductive agent cannot be separated out, so that dispersants will be present in the pole pieces when the positive and negative electrodes are assembled. The presence of these dispersants will reduce the high-voltage resistance of the battery after the pole pieces are assembled into batteries. The fundamental reason is that dispersants are often some polymer or small molecule materials, which will decompose under high voltage and high current to produce gas and cause cyclic expansion and other undesirable phenomena. Therefore, it is difficult to apply to charging and discharging under high current. In the fast-paced pace of life, this type of graphene conductive agent is difficult to meet the needs of fast charging.
[0007] Chemical vapor deposition (CVD) is a method of decomposing carbon-containing chemicals (such as methane) at high temperatures. The carbon atoms obtained by the cracking are deposited on the substrate. The carbon atoms combine with carbon atoms to form graphene, which can produce a few or even a single layer of graphene materials. This method is used to prepare transparent graphene films, which can be applied to electronic touch screens, sensors, transistors, etc. The main barrier is how to peel the graphene from the base without damage or pollution, which is still a problem of concern. In addition, the CVD method is not suitable for the preparation of graphene powder materials, and the prepared graphene materials cannot be used as conductive agents in lithium-ion batteries.
[0008] Epitaxial growth, organic synthesis, and carbon tube exfoliation can all produce single-layer and few-layer graphene materials, but their cost and large-scale production are still constraints.
[0009] The redox method uses a chemical method to first oxidize and peel off graphene to obtain high-monolayer graphene oxide (GO), and then reduce GO to obtain graphene. This method is the optimal path to achieve the preparation of high-monolayer graphene powder. Summary of the invention
[0010] To solve the above problems, the present invention provides a method for preparing a few-layer graphene, comprising the following steps:
[0011] S1: Prepare graphene oxide, wherein the graphene oxide satisfies the following conditions:
[0012] The absorption peak of the graphene oxide dispersion with a concentration of 50 ppm at 230 nm is ≥ 2.0;
[0013] S2: preparing a graphene oxide dispersion using the graphene oxide in step S1;
[0014] S3: reducing, separating and drying the graphene oxide dispersion in step S2 to obtain a solid;
[0015] S4: Fluffing the solid obtained in step S3 to obtain a fluffy powder;
[0016] S5: calcining the fluffy powder in step S4 at high temperature to obtain graphene powder.
[0017] Preferably, in step S1, the number of layers of the graphene oxide is ≤3 layers.
[0018] Preferably, the absorption peak of the graphene oxide dispersion with a concentration of 50 ppm at 230 nm is 2.0-3.5, such as 2.1, 2.5, 2.6, 2.8, 3.2, 3.5, etc.
[0019] Preferably, in step S2, the solid content of the graphene oxide dispersion is ≤0.1wt%, more preferably 0.02-0.1wt%, for example 0.02, 0.05, 0.09, 0.1, 0.25, 0.3, 0.35, etc.
[0020] Preferably, the viscosity of the graphene oxide dispersion is ≤1500 mPa·s; more preferably 50-800 mPa·s.
[0021] Preferably, in step S3, the method for reducing the graphene oxide dispersion in step S2 is: reducing it by a redox method.
[0022] Preferably, the reducing agent of the redox method comprises -NH 2 One or more of organic matter, -OH-containing phenols and alcohols, metal hydrides or hydrogen halides, such as monohydric alcohols, polyhydric alcohols, monohydric phenols, polyhydric phenols, NaBH 4 、LiAlH 4 , hydroiodic acid, hydrobromic acid, etc.
[0023] Preferably, the mass ratio of the graphene oxide to the reducing agent is 1:(2-6), for example, 1:2, 1:3, 1:2.5:, 1:3.5, 1:4, 1:5, 1:5.5, 1:6, etc.; more preferably, it is 1:(3-5).
[0024] Preferably, the temperature during the reduction is 50-100° C., and the stirring reaction time is 2-12 h; further preferably, the temperature is 50-80° C., and the stirring reaction time is 8-12 h.
[0025] Preferably, the water content of the solid obtained by drying is ≤5wt%.
[0026] Preferably, the separation method is filtration separation or centrifugal separation.
[0027] Preferably, step S3 further comprises reducing and separating the graphene oxide dispersion in step S2 and then purifying it.
[0028] Preferably, the purification is performed 1-4 times.
[0029] Preferably, in step S4, the fluffing treatment method is: stirring the solid obtained in step S3 in a stirrer.
[0030] Preferably, the stirring speed is 500-2000 rpm, and the stirring time is 0.15-3 h; further preferably, the stirring speed is 1000-2000 rpm, and the stirring time is 0.5-2 h.
[0031] Preferably, the tap density of the fluffy powder is 0.01-0.1 g / cm 3 ; More preferably 0.05-0.09g / cm 3 .
[0032] Preferably, in step S5, the high temperature calcination temperature is 1000-1500°C, and the calcination time is 1-4h; further preferably, the temperature is 1000-1300°C, and the calcination time is 2-4h.
[0033] The invention also protects a graphene powder which is prepared by a preparation method.
[0034] Preferably, the number of layers of the graphene powder is ≤5.
[0035] The working principle of the present invention is: GO raw materials are prepared in batches by the improved Hummers method, and then a thin layer of GO is obtained by reducing the concentration of GO in water to achieve the effect of reducing agglomeration after reduction; after reduction by chemical reagents, the obtained rGO is separated, and the rGO at this time can be stably dispersed in water; rGO powder is obtained after drying. At this time, if it is simply dried, rGO agglomerates will be obtained, so the rGO powder is stirred at high speed in a closed container for fluffing treatment to achieve the effect of breaking up, preventing the dried rGO powder from agglomerating together, and obtaining a thin layer of rGO powder; finally, this thin layer of rGO is directly repaired at high temperature to obtain a powder material of a few-layer graphene. In the above process, by controlling the preparation of the thin layer of rGO and the fluffing of the rGO powder, the rGO powder before high-temperature repair can achieve the effect of a thin layer, and then a few-layer graphene powder is prepared by high-temperature repair, so as to achieve the macro-scale preparation of graphene powder and meet the requirements of downstream applications.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The development of graphene powder materials has made up for the gap between the conductivity of graphene powder on the market and theoretical graphene, and further enhanced the practical application value of graphene;
[0038] (2) It provides favorable support for lithium batteries to achieve high energy density and faster charging performance;
[0039] (3) Realize the large-scale preparation of graphene powder to meet the requirements of downstream applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0041] Figure 1 is a schematic diagram of a method for preparing graphene provided by the present invention;
[0042] Figure 2 is an atomic force microscope image of the raw material GO in an embodiment of the present invention;
[0043] Figure 3 is a scanning electron microscope image of graphene obtained by the preparation method of an embodiment of the present invention;
[0044] Figure 4 It is a transmission electron microscope image of graphene obtained by the preparation method of the embodiment of the present invention. DETAILED DESCRIPTION
[0045] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0047] This article relates to numerical ranges. Unless otherwise specified, the above numerical ranges are considered continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0048] The temperature parameters herein, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows for temperature fluctuations within the precision range of instrument control.
[0049] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0050] like Figure 1 It is a schematic diagram of the method for preparing few-layer graphene provided by the present invention.
[0051] The present invention provides a method for preparing a few-layer graphene, comprising the following steps:
[0052] (1) Selection of raw material GO
[0053] In order to achieve good dispersion of GO at a solid content of ≤0.1%, GO itself needs to be easily dispersed, so the monolayer rate of GO itself needs to be relatively high. At the same time, GO has a high affinity with water, so the raw material GO needs to have a high degree of oxidation and a high degree of exfoliation.
[0054] In order to select the GO raw material with a lower number of layers that meets the requirements, the method used is to test the solubility of GO in water, specifically: GO is dispersed in water to obtain a dispersion with a concentration of 50ppm, and the absorption peak of the dispersion at 230nm is tested by UV-vis (ultraviolet visible absorption spectrometer). When the absorption peak is ≥2.0, GO can be well dispersed in water to a lower number of layers; preferably, the absorption peak range is 2.0-3.5. In the present invention, the number of layers of GO after dispersion is ≤3 layers.
[0055] In order to further confirm whether the selected raw material GO is low-layered, the raw material can also be tested by atomic force microscopy, such as Figure 2 As shown in the figure, it can be seen that the raw material GO is basically in a single-layer state.
[0056] In the present invention, the number of layers of the raw material GO refers to the number of layers when the raw material GO is dispersed in a dispersion liquid with a concentration of 50 ppm.
[0057] (2) Preparation of low concentration GO dispersion
[0058] GO is prepared into an aqueous dispersion with a solid content of ≤0.1wt%, preferably, the solid content is 0.02-0.1wt%. The GO dispersion is prepared into a dispersion with a viscosity of ≤1500mPa·s, preferably, the viscosity is 50-800mPa·s, by means of stirring dispersion, homogenous dispersion, microfluidization, etc., to ensure that GO can be evenly dispersed in the aqueous solution.
[0059] The solid content mentioned above refers to the mass percentage of the remaining part of the emulsion or coating after drying under specified conditions.
[0060] When the solid content is greater than 0.1%, the aqueous dispersion prepared by GO is not easy to disperse into a single layer or a few layers. When the reduction is carried out, the sheets are easy to agglomerate, which easily leads to the number of layers of the prepared rGO being higher than 5, and the few-layer graphene cannot be obtained. When the solid content is ≤0.1%, the viscosity is ≤1500mPa·s. If the viscosity is too high, the reducing agent added later will react unevenly.
[0061] (3) Reduction of GO dispersion
[0062] Add a chemical reducing agent to the GO dispersion, the mass ratio of GO solid to chemical reducing agent is 1: (2-6); preferably, 1: (3-5). Stir the reaction at a temperature of 50-100°C for 2-12 hours to obtain a black flocculent liquid, and separate the black solid; preferably, the temperature is 50-80°C and the stirring reaction time is 8-12 hours. The black solid is washed with water 1-4 times for purification.
[0063] When the mass ratio of GO solid to chemical reducing agent is less than 1:2, GO is not completely reduced, which will lead to incomplete repair during subsequent high-temperature repair. At the same time, the rGO agglomeration effect is more obvious because the hydrogen bonding force between GO will accelerate the agglomeration. When it is higher than 1:6, in addition to the waste of resources, excessive reducing agent will remain on rGO. The addition of excessive reducing agent to GO solution will lead to GO agglomeration, and few-layer graphene materials cannot be prepared.
[0064] When the temperature is lower than 50°C, the reduction effect will be reduced; when the temperature is too high, GO or rGO (redox graphene) in the obtained solution will agglomerate.
[0065] When the stirring time is 2-12 hours, the reaction can be fully carried out within this time period. If it is longer than this time, it will lead to energy waste and reduced efficiency.
[0066] Among them, the chemical reducing agent includes -NH 2Organic matter, phenols and alcohols containing -OH (monohydric alcohols, polyhydric alcohols, monohydric phenols, polyhydric phenols), metal hydrides (NaBH 4 、LiAlH 4 etc.), hydrogen halides (hydroiodic acid, hydrobromic acid), etc., can be a mixture of one or more of the above chemical reducing agents, and can be selected according to actual needs.
[0067] There are many methods for separating the black flocculent liquid to obtain the black solid, such as filtration separation, centrifugal separation, etc. As long as the method can achieve the separation purpose, it is not limited here.
[0068] (4) Drying and fluffing the purified black solid
[0069] The purified black solid was dried in an oven to obtain rGO powder. The water content of the dried solid was ≤5wt%.
[0070] When the water content of the solids is within the above range, the solids are in block form and can be fully fluffed during subsequent high-speed stirring. When the water content is higher than 5wt%, the solids may stick to the stirring device and cannot be fully fluffed to achieve the purpose of fluffing.
[0071] Stir in a high-speed stirrer, for example, using the stirring device in patent CN213611236U, the stirring speed is 500-2000rpm, the stirring time is 0.15-3h, preferably, the stirring speed is 1000-2000rpm, and the stirring time is 0.5-2h. Within the above range, the solid can be fully fluffed, so that the rGO is dispersed as much as possible, preparing for the subsequent high-temperature graphitization treatment to obtain a graphene powder with a number of layers ≤5 layers. Using the principle of stirring convection, the dried rGO black agglomerates are stirred and fluffed, and the tap density of the rGO black agglomerates before the fluffing treatment is 0.1-0.4g / cm 3 After the fluffing treatment, the tap density of the fluffy rGO powder is 0.01-0.1g / cm 3 , preferably 0.05 to 0.09 g / cm 3 .
[0072] Tap density refers to the mass per unit volume of powder in a container measured after being tapped under specified conditions.
[0073] (5) High temperature repair of fluffy rGO powder to obtain graphene powder
[0074] The fluffy rGO powder is placed in a high temperature furnace in an inert environment for calcination, the temperature is raised to 1000-1500°C at 5°C / min, and the heat treatment is performed for 1-4 hours to obtain a powder material of a few-layer graphene; preferably, the temperature is 1000-1300°C and the calcination time is 2-4 hours. Figure 3 , Figure 4 shown.
[0075] When the temperature is lower than 1000℃, it is not enough to completely eliminate the oxygen-containing functional groups on rGO, so the defects caused by O atoms cannot be completely repaired; when the temperature is higher than 1500℃, a rearrangement reaction of C atoms will occur, and a two-dimensional graphene sheet structure with a complete lattice will be repaired. At this time, overlap occurs between the graphene sheets (due to π-π forces).
[0076] The graphene powder prepared by the above preparation method is tested, and the test method is as follows:
[0077] The test method for the mass fraction of element C and element O is: DB32 / T 3595-2019.
[0078] The test method for ID / IG is: Q / NGSIC 012-2020.
[0079] The test method for specific surface area (BET) is: GBT 7702.20-1997.
[0080] The test method for oil absorption value is: GBT 3780.2-2007.
[0081] The conductivity test method is: Sasha Stankovich, Dmitriy A. Dikin, et al., Synthesis of graphene-based nanosheets via chemical reduction of exfoliated graphite oxide, Carbon 45 (2007): [lines 1558-1565]. The conductivity of graphene powder is tested by the method in this document.
[0082] The test results are shown in Table 1.
[0083] Table 1 Performance data of graphene powder prepared by the preparation method of the present invention
[0084]
[0085] From the data in Table 1, we can see that C (wt%) ≥ 97.2%, O (wt%) ≤ 0.05%, indicating that the GO raw material is basically completely reduced to generate graphene; ID / IG ≤ 1.05 indicates that the defect degree of graphene after thermal repair is low; BET ≥ 750m 2 / g shows that the specific surface area of graphene prepared by this method is relatively large. At the same time, according to the theoretical specific surface area of graphene, when the specific surface area is 750m 2 / g, the average number of graphene layers is about 3. This shows that the BET of graphene powder is ≥750m 2 / g is a few-layer graphene; the oil absorption value is between 3500 and 5500 ml / 100 g, which shows that the graphene powder material has a large specific surface area. The larger the oil absorption value, the larger the specific surface area, and vice versa; the conductivity range is 10 5 ~10 6 S / m shows that the prepared graphene powder has good conductivity.
[0086] The present invention is further described below in conjunction with specific embodiments.
[0087] Embodiment 1:
[0088] A method for preparing graphene powder:
[0089] Prepare GO raw materials with a layer number of ≤3 layers (a dispersion obtained by dispersing GO in water, with a concentration of 50ppm and an absorption peak of 2.08 at 230nm), take 5g of an aqueous dispersion with a GO solid content of 0.05%, stir evenly, add 15g of vitamin C, heat to 80°C, continue stirring for 5h, and then separate the obtained reaction solution to obtain reduced rGO. After washing with water twice, dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1500rpm for 30min to obtain fluffy black rGO powder. Place the black rGO powder in a high-temperature calcining furnace under a nitrogen environment, raise the temperature to 1000°C at a heating rate of 5°C / min, and heat treat for 4h to obtain graphene powder. The performance of the graphene powder was tested, see Table 2.
[0090] Embodiment 2:
[0091] A method for preparing graphene powder:
[0092] Prepare GO raw materials with ≤3 layers (the dispersion obtained by dispersing GO in water has a concentration of 50ppm and an absorption peak of 2.06 at 230nm), take 5g of an aqueous dispersion with a GO solid content of 0.02%, stir evenly, add 10g of ethylenediamine, heat to 50°C, continue stirring for 3h, and then separate the obtained reaction solution to obtain reduced rGO. After washing with water twice, dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1000rpm for 30min to obtain fluffy black rGO powder. Place the black rGO powder in a high-temperature calcining furnace under a nitrogen environment, raise the temperature to 1100°C at a heating rate of 5°C / min, and heat treat for 3h to obtain graphene powder. The performance of the graphene powder was tested, see Table 2.
[0093] Embodiment 3:
[0094] A method for preparing graphene powder:
[0095] Prepare GO raw materials with a layer number of ≤3 layers (a dispersion obtained by dispersing GO in water, with a concentration of 50ppm and an absorption peak of 2.07 at 230nm), take 5g of an aqueous dispersion with a GO solid content of 0.1%, stir evenly, add 10g of vitamin C, heat to 65°C, continue stirring for 8h, and then separate the obtained reaction solution to obtain reduced rGO. After washing with water twice, dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1500rpm for 30min to obtain fluffy black rGO powder. Place the black rGO powder in a high-temperature calcining furnace under a nitrogen environment, raise the temperature to 1400°C at a heating rate of 5°C / min, and heat treat for 2h to obtain graphene powder. The performance of the graphene powder was tested, see Table 2.
[0096] Embodiment 4:
[0097] A method for preparing graphene powder:
[0098] Prepare GO raw materials with a layer number of ≤3 layers (a dispersion obtained by dispersing GO in water, with a concentration of 50ppm and an absorption peak of 2.12 at 230nm), take 5g of an aqueous dispersion with a GO solid content of 0.01%, stir evenly, add 23g of vitamin C, heat to 95°C, continue stirring for 2h, and then separate the obtained reaction solution to obtain reduced rGO. After washing with water twice, dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1500rpm for 30min to obtain fluffy black rGO powder. Place the black rGO powder in a high-temperature calcining furnace under a nitrogen environment, raise the temperature to 1500°C at a heating rate of 5°C / min, and heat treat for 1h to obtain graphene powder. The performance of the graphene powder was tested, see Table 2.
[0099] Embodiment 5:
[0100] A method for preparing graphene powder:
[0101] Prepare GO raw materials with a layer number of ≤3 layers (a dispersion obtained by dispersing GO in water, with a concentration of 50ppm and an absorption peak of 2.14 at 230nm), take 5g of an aqueous dispersion with a GO solid content of 0.01%, stir evenly, add 10g of hydroiodic acid, heat to 50°C, continue stirring for 2h, and then separate the obtained reaction solution to obtain reduced rGO. After washing with water twice, dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1000rpm for 30min to obtain fluffy black rGO powder. Place the black rGO powder in a high-temperature calcining furnace under a nitrogen environment, raise the temperature to 1300°C at a heating rate of 5°C / min, and heat treat for 2.5h to obtain graphene powder. The performance of the graphene powder was tested, see Table 2.
[0102] Comparative Example 1:
[0103] A method for preparing graphene powder:
[0104] Prepare GO raw materials with more than 3 layers (a dispersion obtained by dispersing GO in water, with a concentration of 50ppm and an absorption peak of 1.03 at 230nm), take 5g of an aqueous dispersion with a GO solid content of 0.05%, stir evenly, add 15g of Vc (vitamin C), heat to 80°C, continue stirring for 5h, and then separate the obtained reaction solution to obtain reduced rGO. After washing with water twice, dry in an oven to obtain a solid. Place the solid in a high-speed disperser and stir at 1500rpm for 30min to obtain fluffy black rGO powder. Place the black rGO powder in a high-temperature calcining furnace under a nitrogen environment, raise the temperature to 1300°C at a heating rate of 5°C / min, and heat treat for 2.5h to obtain graphene powder. The performance of the graphene powder was tested, see Table 2.
[0105] Comparative Example 2:
[0106] A method for preparing graphene powder:
[0107] Prepare GO raw materials with a layer number of ≤3 layers (the dispersion obtained by dispersing GO in water has a concentration of 50ppm and an absorption peak of 2.08 at 230nm), take 5g of an aqueous dispersion with a GO solid content of 0.05%, stir evenly, add 15g of Vc (vitamin C), heat to 80°C, continue stirring for 5h, and then separate the obtained reaction solution to obtain reduced rGO. After washing with water twice, dry in an oven to obtain a solid. The black rGO solid was placed in a high-temperature calcining furnace under a nitrogen environment, the temperature was raised to 1300°C at a heating rate of 5°C / min, and heat treated for 2.5h to obtain graphene powder. The performance of the graphene powder was tested, see Table 2.
[0108] Comparative Example 3:
[0109] A method for preparing graphene powder:
[0110] Prepare GO raw materials with more than 3 layers (the dispersion obtained by dispersing GO in water has a concentration of 50ppm and an absorption peak of 1.03 at 230nm), take 5g of an aqueous dispersion with a GO solid content of 0.05%, stir evenly, add 15g of Vc (vitamin C), heat to 80°C, continue stirring for 5h, and then separate the obtained reaction solution to obtain reduced rGO. After washing with water twice, dry in an oven to obtain a solid. The black rGO solid was placed in a high-temperature calcination furnace under a nitrogen environment, the temperature was raised to 1300°C at a heating rate of 5°C / min, and heat treated for 2.5h to obtain graphene powder. The performance of the graphene powder was tested, see Table 2.
[0111] Table 2 Performance data of graphene prepared in the examples and comparative examples
[0112]
[0113]
[0114] Comparison of Example 1 with Comparative Example 1 shows that when the number of layers of the raw material GO is greater than 3, the specific surface area of the obtained graphene powder is significantly lower than that of the graphene with a low layer (≤3 layers) of the raw material GO, and a few-layer graphene material cannot be made.
[0115] Compared with Example 2, when the rGO obtained in the intermediate process is not subjected to a fluffy treatment, graphene powder with a high specific surface area cannot be obtained.
[0116] Compared with Example 3, when the number of layers of the raw material GO is not controlled and the rGO obtained in the intermediate process is not fluffed, the specific surface area of the obtained graphene powder material is lower, and graphene powder with a high specific surface area cannot be obtained.
[0117] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0118] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing graphene powder, characterized in that: The steps include: S1: Prepare graphene oxide, wherein the graphene oxide satisfies the following conditions: The absorption peak of the graphene oxide dispersion with a concentration of 50 ppm at 230 nm is ≥ 2.0; S2: preparing a graphene oxide dispersion using the graphene oxide in step S1; S3: reducing, separating and drying the graphene oxide dispersion in step S2 to obtain a solid; S4: Fluffing the solid obtained in step S3 to obtain a fluffy powder; S5: calcining the fluffy powder obtained in step S4 at high temperature to obtain graphene powder.
2. The preparation method according to claim 1, characterized in that: In step S1, the number of layers of the graphene oxide is ≤3; Preferably, the absorption peak of the graphene oxide dispersion with a concentration of 50 ppm at 230 nm is 2.0-3.
5.
3. The preparation method according to claim 1, characterized in that: In step S2, the solid content of the graphene oxide dispersion is ≤0.1wt%; preferably, 0.02-0.1wt%.
4. The preparation method according to claim 3, characterized in that: The viscosity of the graphene oxide dispersion is ≤1500 mPa·s, preferably 50-800 mPa·s.
5. The preparation method according to claim 1, characterized in that: In step S3, the method for reducing the graphene oxide dispersion in step S2 is: reducing by a redox method; Preferably, the reducing agent used in the redox method is one or more of an organic substance containing -NH2, a phenol and an alcohol containing -OH, a metal hydride or a hydrogen halide; Preferably, the mass ratio of the graphene oxide to the reducing agent is 1:(2-6); more preferably 1:(3-5); Preferably, the temperature during the reduction is 50-100°C, and the stirring reaction time is 2-12h; more preferably, the temperature is 50-80°C, and the stirring reaction time is 8-12h; Preferably, the water content of the solid obtained by drying is ≤5wt%.
6. The preparation method according to claim 1, characterized in that: The separation method is filtration separation or centrifugal separation.
7. The preparation method according to claim 1, characterized in that: Step S3 also includes reducing and separating the graphene oxide dispersion in step S2 and then purifying it; Preferably, the purification is performed 1-4 times.
8. The preparation method according to claim 1, characterized in that: In step S4, the fluffing treatment method is: stirring the solid obtained in step S3 in a stirrer; Preferably, the stirring speed is 500-2000 rpm, and the stirring time is 0.15-3 h; more preferably, the stirring speed is 1000-2000 rpm, and the stirring time is 0.5-2 h; Preferably, the tap density of the fluffy powder is 0.01-0.1 g / cm 3 ; More preferably 0.05-0.09g / cm 3 .
9. The preparation method according to claim 1, characterized in that: In step S5, the high temperature calcination temperature is 1000-1500°C, and the calcination time is 1-4h; Preferably, the temperature is 1000-1300° C. and the calcination time is 2-4 hours.
10. A graphene powder, characterized in that: Prepared by any preparation method of claims 1-9; Preferably, the number of layers of the graphene powder is ≤5.
Citation Information
Patent Citations
Mixing granulation equipment
CN213611236U
Preparing method of oxidized graphene and high-conductivity graphene
CN106564891A
Preparation method for single-layer graphene dispersion liquid
CN107857257A
Quantitative characterization method for dispersion degree of graphene oxide and characterization model for dispersion degree of graphene oxide
CN108693129A
Graphene preparation method, graphene powder and product
CN114590799A