Single-layer Ti3C2-MXene material as well as preparation method and application thereof

The single-layer Ti3C2-MXene material was prepared by treating titanium aluminum carbide by etching solution, which solved the adsorption and detection of SF6 decomposition components in gas insulated transformers, and achieved high response sensitivity adsorption to CF4 and C2F6, ensuring equipment stability.

CN118908214APending Publication Date: 2024-11-08LISHUI POWER SUPPLY COMPANY OF STATE GRID ZHEJIANG ELECTRIC POWER +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410973109.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The strong greenhouse gas SF6 used in existing gas insulating transformers is decomposed into carbon tetrafluoride and hexafluoroethane during partial discharge, resulting in reduced insulation performance, threatening the stability of the equipment, and lacking effective adsorption and detection methods.

Method used

Single-layer Ti3C2-MXene material was prepared by treating titanium aluminum carbide (Ti3AlC2) by etching solution, controlling its etching degree to improve the adsorption effect of perfluoroisobutyronitrile decomposition components, and used to prepare sensors, detect carbon tetrafluoride and Decomposition components of hexafluoroethane.

Benefits of technology

High-response sensitivity adsorption of perfluoroisobutyronitrile decomposition components CF4 and C2F6 is achieved, which improves the response capability of the detection sensor and ensures the stable operation of the gas insulated transformer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908214A_ABST
    Figure CN118908214A_ABST
Patent Text Reader

Abstract

The invention discloses a single-layer Ti3C2-MXene material as well as a preparation method and application thereof, and the preparation method comprises the following steps: S1, etching titanium aluminum carbide by using an etching solution to obtain a Ti3C2-MXene material with a multi-layer structure; s2, carrying out intercalation treatment on the Ti3C2-MXene material with the multilayer structure by using an organic solvent, then carrying out solid-liquid separation, and carrying out ultrasonic layering treatment on the solid to obtain a single-layer Ti3C2-MXene material; the solid-to-liquid ratio of the titanium aluminum carbide to the etching solution is 2g: (38-42) mL; the etching solution contains hydrochloric acid and metal fluoride, and the mass fraction concentration of the hydrochloric acid is 16%-21%; the mass concentration of the metal fluoride is 0.04 to 0.06 g / mL. The single-layer Ti3C2-MXene material capable of adsorbing decomposition components of perfluoroisobutyronitrile is obtained by regulating and controlling the etching degree of titanium aluminum carbide, and the sensor is prepared from the single-layer Ti3C2-MXene material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of inorganic materials, and more specifically, to a single-layer Ti3C2-MXene material and a preparation method and application thereof. Background Art

[0002] Gas insulated equipment (GIE) has the advantages of small footprint, high reliability, and long dimensional cycle, and plays an important role in the power transmission and distribution systems of various voltage levels. Gas insulated equipment mainly includes gas insulated switchgear (GIS), gas insulated line (GIL), gas insulated transformer (GIT) and gas insulated cabinet (GIC). Gas insulated transformer is an important component of gas insulated equipment, which is mostly filled with high pressure (0.13-0.6MPa) sulfur hexafluoride (SF6) gas as insulation or arc extinguishing medium. However, SF6 is an extremely strong greenhouse gas, with a global warming potential (GWP) of 23,500 times that of CO2 and an atmospheric lifetime of 3,200 years. It was listed as one of the six major greenhouse gases in the Kyoto Protocol in 1997. At present, the use of SF6 in the global power industry accounts for 80% of its annual production. Therefore, there is an urgent need to find an environmentally friendly gas insulation medium for use in gas-insulated transformers to comply with the green and low-carbon development concept. At the same time, this can also solve the global power industry's dependence on the strong greenhouse gas SF6.

[0003] Perfluoroisobutyronitrile (C4F7N) is an environmentally friendly gas insulation medium that replaces the strong greenhouse gas SF6 and has excellent insulation tolerance. When insulation faults such as partial discharge occur in gas-insulated transformers, perfluoroisobutyronitrile (C4F7N) will decompose into carbon tetrafluoride (CF4) and hexafluoroethane (C2F6), which will reduce the insulation performance of the gas-insulated transformer and threaten the normal operation and stability of the equipment. Therefore, it is urgent to determine whether perfluoroisobutyronitrile (C4F7N) has decomposed by adsorbing and detecting the decomposition components of perfluoroisobutyronitrile (C4F7N).

[0004] Therefore, it is of great significance to develop a preparation method for a single-layer Ti3C2-MXene material that can adsorb the decomposition components of perfluoroisobutyronitrile. Summary of the invention

[0005] The object of the present invention is to provide a single-layer Ti3C2-MXene material capable of adsorbing decomposition components of perfluoroisobutyronitrile, and a preparation method and application thereof.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] In a first aspect, the present invention provides a method for preparing a single-layer Ti3C2-MXene material, comprising the following steps:

[0008] S1. Etching titanium aluminum carbide (Ti3AlC2) with an etching solution to obtain a Ti3C2-MXene material having a multilayer structure;

[0009] S2. The Ti3C2-MXene material having a multilayer structure is intercalated with an organic solvent, and then the solid-liquid is separated and the solid is ultrasonically layered to obtain a single-layer Ti3C2-MXene material;

[0010] In step S1, the solid-liquid ratio of the titanium aluminum carbide (Ti3AlC2) and the etching solution is 2g:(38-42)mL; the etching solution contains hydrochloric acid and metal fluoride, the mass fraction concentration of the hydrochloric acid is 16%-21%; the mass concentration of the metal fluoride is 0.04-0.06g / mL.

[0011] The present invention adjusts the etching degree of titanium aluminum carbide (Ti3AlC2) by controlling the solid-liquid ratio of titanium aluminum carbide (Ti3AlC2) and an etching solution, and the concentrations of hydrochloric acid and metal fluoride in the etching solution, thereby obtaining a single-layer Ti3C2-MXene material having an adsorption effect on the decomposition components of perfluoroisobutyronitrile, and further making a sensor for detecting the decomposition components of perfluoroisobutyronitrile prepared by using the single-layer Ti3C2-MXene material have good response sensitivity to the decomposition components CF4 and C2F6 of perfluoroisobutyronitrile.

[0012] Specifically, when the solid-liquid ratio of titanium aluminum carbide (Ti3AlC2) and the etching solution is too small, and / or the concentration of hydrochloric acid and metal fluoride in the etching solution is too large, the degree of etching of titanium aluminum carbide (Ti3AlC2) is relatively serious, the structure is severely damaged, and the number of adsorption sites of the single-layer Ti3C2-MXene material decreases, resulting in the single-layer Ti3C2-MXene material. The adsorption effect of the decomposition components of perfluoroisobutyronitrile becomes worse, and the response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile prepared using the single-layer Ti3C2-MXene material decreases.

[0013] When the solid-to-liquid ratio of titanium aluminum carbide (Ti3AlC2) and the etching solution is too large, and / or the concentrations of hydrochloric acid and metal fluoride in the etching solution are too small, the etching degree of titanium aluminum carbide (Ti3AlC2) is insufficient, a large number of Al atoms are not etched away, and sufficient adsorption sites cannot be generated, resulting in poor adsorption effect of the single-layer Ti3C2-MXene material on the decomposition components of perfluoroisobutyronitrile, which in turn leads to a decrease in the response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile prepared using the single-layer Ti3C2-MXene material.

[0014] Preferably, the mass fraction concentration of the hydrochloric acid is 16.65%-20.35%; the mass concentration of the metal fluoride is 0.045-0.055 g / mL.

[0015] Preferably, in step S1, the etching temperature is 50-80° C. and the etching time is 44-52 h.

[0016] More preferably, in step S1, the etching temperature is 50-70°C.

[0017] In the present invention, the etching degree of titanium aluminum carbide (Ti3AlC2) can be more effectively controlled by controlling the etching temperature, which can further improve the adsorption effect of the single-layer Ti3C2-MXene material on the decomposition components of perfluoroisobutyronitrile, thereby further improving the response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile prepared using the single-layer Ti3C2-MXene material.

[0018] Preferably, in step S1, the metal fluoride is at least one of sodium fluoride (NaF) and lithium fluoride (LiF).

[0019] In the present invention, titanium aluminum carbide (Ti3AlC2) can be prepared according to methods known in the art, or obtained through commercial channels.

[0020] The present invention provides a method for preparing titanium aluminum carbide (Ti3AlC2), comprising:

[0021] Titanium hydride (TiH2), aluminum powder (Al powder) and carbon powder (C powder) are heated to obtain titanium aluminum carbide (Ti3AlC2);

[0022] The heating temperature is 1400-1500° C. and the heating time is 2-3 hours.

[0023] Preferably, the heating temperature is 1400° C. and the heating time is 2 hours.

[0024] Preferably, in step S2, the organic solvent is dimethyl sulfoxide (DMSO).

[0025] Preferably, in step S2, the intercalation treatment is to place the Ti3C2-MXene material having a multilayer structure in an organic solvent and stir it.

[0026] Preferably, in step S2, the temperature of the intercalation treatment is 20-40°C and the time is 16-20 hours.

[0027] Preferably, in step S2, during the ultrasonic stratification treatment, the liquid environment that the solid directly contacts is at least one of water, ethanol and dimethyl sulfoxide (DMSO).

[0028] Preferably, in step S2, the temperature of the ultrasonic stratification treatment is 20-40°C and the time is 5-7h.

[0029] Preferably, in step S2, the ultrasonic stratification treatment is performed in an inert gas environment; the inert gas is at least one of nitrogen, argon, helium, and a helium-nitrogen mixture.

[0030] In a second aspect, the present invention provides a single-layer Ti3C2-MXene material prepared by the above-mentioned preparation method.

[0031] In a third aspect, the present invention provides an application of a single-layer Ti3C2-MXene material in the adsorption of decomposition components of perfluoroisobutyronitrile.

[0032] Preferably, the perfluoroisobutyronitrile decomposition component is at least one of carbon tetrafluoride (CF4) and hexafluoroethane (C2F6).

[0033] In a fourth aspect, the present invention provides a sensor for detecting decomposition components of perfluoroisobutyronitrile, comprising:

[0034] An interdigitated electrode coated with a single layer of Ti3C2-MXene material, and a resistance detection device connected to the interdigitated electrode.

[0035] Preferably, the interdigitated electrodes are placed on a carrier.

[0036] More preferably, the carrier is a ceramic tube; specifically, the ceramic tube has an outer diameter of 1-2 mm, an inner diameter of 0.5-1.5 mm, and a length of 2-8 mm.

[0037] More preferably, the ceramic tube has an outer diameter of 1.2 mm, an inner diameter of 0.8 mm, and a length of 4 mm.

[0038] Preferably, the coating amount of the single layer Ti3C2-MXene material on the interdigitated electrode is 35-40 mg / cm 2 .

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The method for preparing a single-layer Ti3C2-MXene material of the present invention regulates the etching degree of titanium aluminum carbide (Ti3AlC2) by controlling the solid-to-liquid ratio of titanium aluminum carbide (Ti3AlC2) and an etching solution, and the concentrations of hydrochloric acid and metal fluoride in the etching solution, so as to obtain a single-layer Ti3C2-MXene material having an adsorption effect on decomposition components of perfluoroisobutyronitrile, thereby making a sensor for detecting decomposition components of perfluoroisobutyronitrile prepared by using the single-layer Ti3C2-MXene material have good response sensitivity to the decomposition components CF4 and C2F6 of perfluoroisobutyronitrile.

[0041] In the preparation method of the single-layer Ti3C2-MXene material of the present invention, the etching degree of titanium aluminum carbide (Ti3AlC2) can be more effectively controlled by controlling the etching temperature, which can further improve the adsorption effect of the single-layer Ti3C2-MXene material on the decomposition components of perfluoroisobutyronitrile, thereby further improving the response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile prepared using the single-layer Ti3C2-MXene material. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is the SEM image of the Ti3C2-MXene material with a multilayer structure in Example 1.

[0043] Figure 2 This is the SEM image of the Ti3C2-MXene material with a multilayer structure in Example 1.

[0044] Figure 3 A schematic diagram of a partial structure of a sensor for detecting decomposition components of perfluoroisobutyronitrile, wherein: 1- interdigitated electrode, 2- ceramic tube.

[0045] Figure 4 This is a time-response sensitivity curve of the sensor for detecting the decomposition components of perfluoroisobutyronitrile to CF4 in Application Example 1.

[0046] Figure 5 This is a standard curve of the concentration-response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile to CF4 in Application Example 1.

[0047] Figure 6 This is the time-response sensitivity curve of the sensor for detecting the decomposition components of perfluoroisobutyronitrile to C2F6 in Application Example 1.

[0048] Figure 7 This is a standard curve of the concentration-response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile to C2F6 in Application Example 1. DETAILED DESCRIPTION

[0049] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0050] Example 1

[0051] This embodiment provides a single-layer Ti3C2-MXene material, and a preparation method thereof comprises the following steps:

[0052] S1. A method for preparing titanium aluminum carbide (Ti3AlC2), comprising: heating 3 g of titanium hydride (TiH2), 1.5 g of aluminum powder (Al powder) and 1 g of carbon powder (C powder) at 1400°C in a tube furnace for 4 h to obtain titanium aluminum carbide (Ti3AlC2);

[0053] S2. Take 20 mL of 37% commercially available concentrated hydrochloric acid and 2 g of sodium fluoride and add them to deionized water to obtain an etching solution with a volume of 40 mL;

[0054] S3. Grind titanium aluminum carbide (Ti3AlC2) into powder, pass through a 500-mesh sieve (<25 μm), take 2 g and put it into 40 mL etching solution, stir and etch at 60 ° C for 48 h, then wash with deionized water for several times until the pH of the supernatant is 6, then wash with anhydrous ethanol for 3 times, and vacuum dry at 60 ° C to obtain a Ti3C2-MXene material with a multilayer structure, such as Figure 1-2 As shown;

[0055] S4. Take 0.25g of Ti3C2-MXene material with a multilayer structure and add it to 10mL of dimethyl sulfoxide (DMSO), stir it at 25°C for 18h for intercalation treatment, then centrifuge it at 8000rpm for 10min for solid-liquid separation, place the solid obtained by centrifugation in 70mL of deionized water, and ultrasonically layer it in a flowing inert gas nitrogen environment at 25°C for 6h, then centrifuge it at 3500rpm for 1h, take the supernatant, and obtain a single-layer Ti3C2-MXene material;

[0056] In step S3, the solid-liquid ratio of the titanium aluminum carbide (Ti3AlC2) and the etching solution is 2g:40mL; the etching solution contains hydrochloric acid and sodium fluoride (NaF), wherein the mass fraction concentration of the hydrochloric acid is 18.5%; the mass concentration of the sodium fluoride is 0.05g / mL.

[0057] Examples 2-12 and Comparative Examples 1-6

[0058] Examples 2-12 and Comparative Examples 1-6 provide different single-layer Ti3C2-MXene materials and preparation methods thereof, which differ from Example 1 in that the solid-liquid ratio of titanium aluminum carbide (Ti3AlC2) and the etching solution, the mass fraction concentration of hydrochloric acid and the mass concentration of sodium fluoride (NaF) in the etching solution, and the etching temperature of step S3 are different, and the rest are consistent with Example 1, as shown in the following table:

[0059] Table 1 Experimental conditions of Examples 1-12 and Comparative Examples 1-6

[0060]

[0061] Application Examples

[0062] Application Example 1

[0063] This application example provides a sensor for detecting decomposition components of perfluoroisobutyronitrile, including:

[0064] An interdigital electrode coated with a single layer of Ti3C2-MXene material of Example 1, and a resistance detection device connected to the interdigital electrode, and the interdigital electrode is placed on a ceramic tube;

[0065] The coating amount of the single-layer Ti3C2-MXene material of Example 1 on the interdigitated electrode is 36 mg / cm 2 ;

[0066] The ceramic tube has an outer diameter of 1.2 mm, an inner diameter of 0.8 mm, and a length of 4 mm.

[0067] Figure 3 A schematic diagram of a partial structure of a sensor for detecting decomposition components of perfluoroisobutyronitrile, wherein: 1- interdigitated electrode, 2- ceramic tube.

[0068] Application Example 2-12 and Comparative Application Example 1-6

[0069] Application Examples 2-12 and Comparative Application Examples 1-6 provide different sensors for detecting the decomposition components of perfluoroisobutyronitrile. The difference between them and Application Example 1 is that the single-layer Ti3C2-MXene material of Example 2-12 or Comparative Example 1-6 is used to replace the single-layer Ti3C2-MXene material of Application Example 1, and the rest is consistent with Application Example 1.

[0070] Comparative Application Example 7

[0071] This comparative application example provides a sensor for detecting the decomposition components of perfluoroisobutyronitrile. The only difference between this sensor and application example 1 is that the Ti3C2-MXene material with a multilayer structure prepared in step S3 of embodiment 1 is used to replace the single-layer Ti3C2-MXene material of application example 1, and the rest is consistent with application example 1.

[0072] Performance Testing

[0073] The following performance tests were conducted on the sensors for detecting the decomposition components of perfluoroisobutyronitrile in each application example and comparative application example:

[0074] (1) Theoretical test of adsorption energy

[0075] The DFT method is used to simulate and calculate the adsorption energy of the single-layer Ti3C2-MXene material on the decomposition components CF4 and C2F6 of perfluoroisobutyronitrile. The specific experimental steps are as follows:

[0076] S1. Using the Dmol3 module in the Material Studio software, the DFT-D algorithm was used to correct the van der Waals force on the surface of the monolayer Ti3C2-MXene material, and the generalized gradient approximation (GGA) method and the Perdew-Burke-Ernzehof (PBE) functional were used to treat the exchange correlation between electrons.

[0077] S2. Enter the following structural optimization setting convergence criteria parameters in Material Studio: the geometric energy difference is less than 1.0×10 -5 Ha, the force on each atom is less than The maximum displacement distance of each atom is less than

[0078] S3. The optimal structural model of the monolayer Ti3C2-MXene material for adsorbing the decomposition components of perfluoroisobutyronitrile, CF4 and C2F6, was established, and the adsorption energy of the monolayer Ti3C2-MXene material for CF4 and C2F6 was calculated, and the adsorption energy calculation formula is as follows:

[0079] E ad =E Ti3C2-MXene+gas -E Ti3C2-MXene -E gas ;

[0080] Among them, E Ti3C2-MXene+gas is the energy of the monolayer Ti3C2-MXene material system after adsorbing CF4 or C2F6 gas, E Ti3C2-MXene is the energy of the monolayer Ti3C2-MXene material system before adsorbing CF4 or C2F6 gas, E gas is the energy of CF4 or C2F6 gas molecules, E ad is the adsorption energy of single-layer Ti3C2-MXene material on CF4 or C2F6;

[0081] Since the adsorption energy E adIt is the energy change value of the monolayer Ti3C2-MXene material system after adsorbing CF4 or C2F6 gas molecules. Therefore, when the adsorption energy is a negative value, it means that the process of adsorbing gas molecules is an exothermic process, and the adsorption is stable; when the adsorption energy is a positive value, it means that the process of adsorbing gas molecules is an endothermic process, and the adsorption is unstable.

[0082] Through calculation, it was found that the adsorption energies of the single-layer Ti3C2-MXene material system for CF4 and C2F6 were -1.26eV and -1.01eV, respectively, indicating that the single-layer Ti3C2-MXene material system may have a good adsorption effect on the decomposition components of perfluoroisobutyronitrile CF4 and / or C2F6.

[0083] Referring to the above method, it was calculated that the adsorption energies of titanium aluminum carbide (Ti3AlC2) for CF4 and C2F6 were -0.277eV and -0.174eV, respectively. When Ti3C2-MXene material was used for adsorption, the adsorption energies were -1.26eV and -1.01eV, indicating that Ti3C2-MXene material may play a catalytic role, making the adsorption effect stronger and further shortening the response and recovery time of the final sensor.

[0084] (2) Response test to carbon tetrafluoride (CF4)

[0085] First, the sensor for detecting the decomposition components of perfluoroisobutyronitrile according to Example 1 was introduced into the C4F7N (perfluoroisobutyronitrile) background gas for 30 minutes, and then CF4 gas with concentrations of 10ppm, 20ppm, 30ppm, 40ppm and 50ppm was introduced respectively, each time for 75 seconds, and after the introduction of CF4 gas of different concentrations, the C4F7N background gas was re-introduced for 175 seconds for recovery, and finally the concentration of CF4 gas was detected by recording the resistance change of the sensor, and the response sensitivity of CF4 gas was calculated by the following formula:

[0086] Response sensitivity of CF4 gas at time t (%) = (test resistance value at time t - initial resistance value) / initial resistance value × 100%;

[0087] The initial resistance value refers to the resistance value displayed by the resistance detection device when C4F7N (perfluoroisobutyronitrile) background gas is introduced for 30 minutes at the beginning, and the test resistance value at time t refers to the resistance value displayed by the resistance detection device when the experiment is carried out to time t.

[0088] Figure 4 This is a time-response sensitivity curve of the sensor for detecting the decomposition components of perfluoroisobutyronitrile to CF4 in Application Example 1. Figure 5 This is a standard curve of the concentration-response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile to CF4 in Application Example 1. Figure 4-5 It can be seen that the response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile in Application Example 1 to 10ppm, 20ppm, 30ppm, 40ppm and 50ppm of CF4 gas is 8.35%, 15.60%, 25.85%, 36.89% and 46.71% respectively, and the concentration-response sensitivity standard curve of the sensor to CF4 is y=0.7326x+1.024, R 2 =0.99346, which shows that the single-layer Ti3C2-MXene material of the present invention has a good response sensitivity to the decomposition component CF4 of perfluoroisobutyronitrile.

[0089] (3) Response test to hexafluoroethane (C2F6)

[0090] First, the sensor for detecting the decomposition components of perfluoroisobutyronitrile according to Example 1 was introduced into the C4F7N (perfluoroisobutyronitrile) background gas for 30 minutes, and then C2F6 gas with concentrations of 10ppm, 20ppm, 30ppm, 40ppm and 50ppm was introduced respectively, each time for 75 seconds, and after the introduction of C2F6 gas of different concentrations, the C4F7N background gas was introduced again for 175 seconds for recovery, and finally the concentration of C2F6 gas was detected by recording the resistance change of the sensor, and the response sensitivity of C2F6 gas was calculated by the following formula:

[0091] Response sensitivity of C2F6 gas at time t (%) = (test resistance value at time t - initial resistance value) / initial resistance value × 100%;

[0092] The initial resistance value refers to the resistance value displayed by the resistance detection device when C4F7N (perfluoroisobutyronitrile) background gas is introduced for 30 minutes at the beginning, and the test resistance value at time t refers to the resistance value displayed by the resistance detection device when the experiment is carried out to time t.

[0093] Figure 6 This is the time-response sensitivity curve of the sensor for detecting the decomposition components of perfluoroisobutyronitrile to C2F6 in Application Example 1. Figure 7 This is a standard curve of the concentration-response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile in Application Example 1 to C2F6. Figure 6-7 It can be seen that the response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile in Application Example 1 to 10ppm, 20ppm, 30ppm, 40ppm and 50ppm of C2F6 gas is 6.42%, 12.01%, 19.88%, 28.37% and 35.93% respectively, and the concentration-response sensitivity standard curve of the sensor to C2F6 is y=0.5635x+0.785, R 2=0.98371, which shows that the single-layer Ti3C2-MXene material of the present invention has a good response sensitivity to the decomposition component C2F6 of perfluoroisobutyronitrile.

[0094] (4) Response test of the sensor for detecting the decomposition components of perfluoroisobutyronitrile in each application example and comparative application example to the decomposition components of perfluoroisobutyronitrile

[0095] First, the sensor for detecting the decomposition components of perfluoroisobutyronitrile in each application example or comparative application example is introduced with C4F7N (perfluoroisobutyronitrile) background gas for 30 minutes, and then the perfluoroisobutyronitrile decomposition component gas to be tested with a concentration of 50ppm is introduced for 75 seconds, and then the C4F7N background gas is re-introduced for 175 seconds for recovery, and finally the perfluoroisobutyronitrile decomposition component gas to be tested is detected by recording the resistance change of the sensor, and the response sensitivity of the perfluoroisobutyronitrile decomposition component gas to be tested is calculated by the following formula:

[0096] Response sensitivity of the decomposition component gas of perfluoroisobutyronitrile to be tested (%) = (test resistance value - initial resistance value) / initial resistance value × 100%;

[0097] The initial resistance value refers to the resistance value displayed by the resistance detection device when C4F7N (perfluoroisobutyronitrile) background gas is introduced for 30 minutes at the beginning, and the test resistance value refers to the resistance value displayed by the resistance detection device after the decomposition component gas of the perfluoroisobutyronitrile to be tested is introduced;

[0098] The decomposition component gas of the perfluoroisobutyronitrile to be tested used in the test is carbon tetrafluoride (CF4) or hexafluoroethane (C2F6);

[0099] The experimental results are as follows:

[0100] Table 2 Test results of sensors in various application examples and comparative application examples

[0101]

[0102]

[0103] As can be seen from Table 2, the present invention controls the etching degree of titanium aluminum carbide (Ti3AlC2) by controlling the solid-liquid ratio of titanium aluminum carbide (Ti3AlC2) and the etching solution, as well as the concentrations of hydrochloric acid and metal fluoride in the etching solution, thereby obtaining a single-layer Ti3C2-MXene material having an adsorption effect on the decomposition components of perfluoroisobutyronitrile, thereby making the sensor for detecting the decomposition components of perfluoroisobutyronitrile prepared using the single-layer Ti3C2-MXene material have a good response sensitivity to the decomposition components of perfluoroisobutyronitrile CF4 and C2F6.

[0104] In the preparation method of the single-layer Ti3C2-MXene material of the present invention, the etching degree of titanium aluminum carbide (Ti3AlC2) can be more effectively controlled by controlling the etching temperature, which can further improve the adsorption effect of the single-layer Ti3C2-MXene material on the decomposition components of perfluoroisobutyronitrile, thereby further improving the response sensitivity of the sensor for detecting the decomposition components of perfluoroisobutyronitrile prepared using the single-layer Ti3C2-MXene material.

[0105] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a single-layer Ti3C2-MXene material, characterized in that: The steps include: S1. Etching titanium aluminum carbide with an etching solution to obtain a Ti3C2-MXene material having a multilayer structure; S2. The Ti3C2-MXene material having a multilayer structure is intercalated with an organic solvent, and then the solid-liquid is separated and the solid is ultrasonically layered to obtain a single-layer Ti3C2-MXene material; In step S1, the solid-liquid ratio of the titanium aluminum carbide and the etching solution is 2g:(38-42)mL; the etching solution contains hydrochloric acid and metal fluoride, the mass fraction concentration of the hydrochloric acid is 16%-21%; the mass concentration of the metal fluoride is 0.04-0.06g / mL.

2. The method for preparing a single-layer Ti3C2-MXene material according to claim 1, characterized in that: The mass fraction concentration of the hydrochloric acid is 16.65%-20.35%.

3. The method for preparing a single-layer Ti3C2-MXene material according to claim 1, characterized in that: The mass concentration of the metal fluoride is 0.045-0.055 g / mL.

4. The method for preparing a single-layer Ti3C2-MXene material according to claim 1, characterized in that: In step S1, the etching temperature is 50-80°C.

5. The method for preparing a single-layer Ti3C2-MXene material as claimed in claim 4, characterized in that: In step S1, the etching temperature is 50-70°C.

6. The method for preparing a single-layer Ti3C2-MXene material according to claim 1, characterized in that: In step S1, the metal fluoride is at least one of sodium fluoride and lithium fluoride.

7. A single-layer Ti3C2-MXene material prepared by the preparation method described in any one of claims 1-6.

8. Use of the single-layer Ti3C2-MXene material according to claim 7 in the adsorption of decomposition components of perfluoroisobutyronitrile.

9. The use according to claim 8, characterized in that The perfluoroisobutyronitrile decomposition component is at least one of carbon tetrafluoride and hexafluoroethane.

10. A sensor for detecting decomposition components of perfluoroisobutyronitrile, characterized in that: include: An interdigital electrode coated with the single-layer Ti3C2-MXene material according to claim 7, and a resistance detection device connected to the interdigital electrode.

Citation Information

Patent Citations

  • Preparation method of single-layer / few-layer MXene two-dimensional material

    CN111285359A

  • Super-elastic and high-adsorbability MXene aerogel and preparation method thereof

    CN114797747A

  • Material structure for biocompatibility of fully-implanted artificial cochlea and preparation of material structure

    CN115607749A

  • Oxygen reduction electrocatalyst based on MXene loaded ZIF as well as preparation method and application of oxygen reduction electrocatalyst

    CN117878341A

  • Water-free etching of max phases into mxenes using organic solvents