Method for deeply removing impurities in high-purity quartz sand under assistance of multi-field coupling

Through multi-field coupling auxiliary methods and cold quenching cleaning, the problem of inability to effectively remove impurities in the quartz sand gas-liquid inclusions in the existing technology is solved, and the efficient depth removal of high-purity quartz sand is achieved, and a green and environmentally friendly cleaning agent is used to improve the It has the efficiency of impurity removal and environmental protection.

CN118908228APending Publication Date: 2024-11-08DALIAN UNIV OF TECH WEST YUNNAN IND DEV RES INST +1

Patent Information

Application Number
CN202410974568.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing high-purity quartz sand impurity depth removal methods cannot effectively remove gas-liquid inclusion impurities in quartz sand, especially when these impurities do not contain high dielectric constant substances, the microwave removal method cannot achieve the removal effect.

Method used

Multi-field coupling auxiliary methods are adopted, including the synergistic effect of ultrasonic field, temperature field, laser field and infrared light field, combined with cold quenching and green and environmentally friendly acid-base cleaning, through preheating, ultrasonic vibration, laser and infrared synchronous processing, cold quenching Cleaning, alkali washing and pickling washing, and other steps to deeply remove gas-liquid inclusion impurities in quartz sand.

Benefits of technology

Through multi-field coupling auxiliary effect and cold quenching cleaning, the probability of quartz sand particles burst is significantly increased, causing the gas-liquid inclusion to overflow from it, achieving efficient deep removal of impurities, and the alkaline wash and pickling wash are green and environmentally friendly. type, in line with current manufacturing philosophy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004954171170000011
    Figure HDA0004954171170000011
  • Figure HDA0004954171170000012
    Figure HDA0004954171170000012
  • Figure HDA0004954171170000021
    Figure HDA0004954171170000021
Patent Text Reader

Abstract

According to the multi-field coupling assisted high-purity quartz sand impurity deep removal method, through the multi-field synergistic effect of a temperature field, an ultrasonic field, an infrared light field and a laser field and the cold quenching effect, the probability that quartz sand particles containing gas-liquid inclusions burst from the interior is increased, and the gas-liquid inclusions are full of the quartz sand and overflow from the quartz sand. And alkali washing and acid washing are assisted by a temperature field, an ultrasonic field and a flow field generated by stirring, so that multi-field coupling effect cleaning is formed, impurities including gas-liquid inclusions are deeply removed, and the impurity removal efficiency is improved. The alkali washing solution and the acid washing solution are green and environment-friendly solutions, do not contain strong acid, strong alkali and toxic substances, do not cause great harm to human bodies and the environment, and conform to the current green manufacturing concept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-purity quartz sand preparation, and in particular to a multi-field coupling-assisted high-purity quartz sand impurity deep removal method. Background Art

[0002] High-purity quartz products have extremely small thermal expansion coefficients, excellent dielectric properties, chemical stability and mechanical strength. They are widely used in semiconductor, photovoltaic, optical communication, military and other industries. They are a key supporting basic material and have an irreplaceable role. Therefore, the use of various sorting and purification methods to separate high-purity quartz sand from quartz sand resources has become a research focus. Quartz sand purification is a hot spot for research and development and investment in the non-metallic mineral industry. The price of quartz sand increases significantly after purification.

[0003] At present, the main methods for deep removal and purification of impurities in high-purity quartz sand include high-temperature calcination, grinding, flotation and acid leaching. It is difficult to remove oxide impurities and ion impurities attached to the surface of quartz sand by high-temperature calcination, grinding, flotation and other methods, and it is difficult to remove gas-liquid inclusion impurities inside quartz by acid leaching. Although some people advocate the use of microwaves to remove gas-liquid inclusion impurities in quartz sand, the impurities in gas-liquid inclusions are diverse. When these impurities do not contain high dielectric constant substances, microwave removal cannot achieve the removal effect. In summary, the existing methods for deep removal of impurities in quartz sand cannot completely remove impurities. Based on this, the present invention proposes a method for deep removal of impurities in high-purity quartz sand assisted by multi-field coupling, which achieves deep removal of impurities in quartz sand including gas-liquid inclusions by multi-field assistance of ultrasonic field, temperature field, laser field and infrared light field, combined with cold quenching and green and environmentally friendly acid-base cleaning. Summary of the invention

[0004] In order to solve the shortcomings of the existing high-purity quartz sand gas-liquid inclusion deep removal, the present invention provides a method for efficiently and stably removing impurities in high-purity quartz sand including gas-liquid inclusion impurities by synergistic assistance of ultrasonic field, temperature field, laser field and infrared light field, combined with cold quenching and green and environmentally friendly acid-base cleaning.

[0005] The technical means adopted by the present invention are as follows:

[0006] A multi-energy field coupling-assisted high-purity quartz sand impurity deep removal method, the specific steps are as follows:

[0007] Step 1, preheating the quartz sand at 400-800°C;

[0008] Step 2, the preheated quartz sand is processed by ultrasonic vibration, laser and infrared synchronously, and the processing time is 3 to 6 hours;

[0009] Step 3, cold quenching and cleaning the quartz sand processed in step 2;

[0010] Step 4, alkali washing and acid washing are respectively performed on the quartz sand after cold quenching and cleaning;

[0011] Step 5: The quartz sand treated in step 4 is cleaned by ultrasonic stirring with anhydrous ethanol, and then dried after cleaning.

[0012] Furthermore, in step 2, the ultrasonic vibration frequency is set to 50 to 100 kHz.

[0013] Furthermore, in step 3, the cold quenching cleaning mechanism adds 3 / 5 volume of deionized water, sets the temperature at 0-5°C, cools the deionized water to 0-5°C, and maintains it; after step 2, transports the quartz sand to the cold extraction cleaning mechanism, pours the quartz sand into the cold extraction cleaning chamber for cold extraction for 30-60 minutes, and at the same time sets the ultrasonic frequency of the cold quenching cleaning mechanism to 20-200kHz, the stirring speed to 20-80r / min, and starts stirring the cold extraction.

[0014] Furthermore, in step 4, after the cold extraction is completed, the quartz sand is taken out, and the deionized water in the cleaning chamber is replaced with a green and environmentally friendly alkaline washing solution. During the alkaline washing process, the temperature is set at 200-400°C, the ultrasonic frequency is set at 20-200kHz, the stirring speed is set at 20-80r / min, and the alkaline washing is started for 5-8 hours.

[0015] Furthermore, the composition of the alkaline washing solution includes the following components in mass concentration units: 50-100 g / L of anhydrous sodium carbonate, 20-80 g / L of guanidine carbonate, and 5-15 vol.% of disodium ethylenediaminetetraacetate.

[0016] Furthermore, in step 4, after the alkaline washing is completed, the quartz sand is taken out, and the alkaline washing liquid in the cleaning chamber is replaced with a green and environmentally friendly acid washing liquid. During the acid washing process, the temperature is set at 200-400°C, the ultrasonic frequency is set at 20-200kHz, the stirring speed is set at 20-80r / min, and the acid washing is started for 5-10 hours.

[0017] Furthermore, the pickling solution composition includes the following components in mass concentration units: malic acid 100-200 g / L, citric acid 80-150 g / L, polyethylene 5-10 vol.%.

[0018] Further, in step 5, after the pickling is completed, the quartz sand is taken out, the pickling liquid in the cleaning chamber is replaced with anhydrous ethanol, the temperature is set to 20-30°C, the ultrasonic frequency is set to 20-200kHz, the stirring speed is set to 20-80r / min, and the cleaning is started for 30-60min;

[0019] After cleaning, use a blower dryer to dry at a temperature of 30 to 50°C.

[0020] The present invention keeps the quartz sand in a high energy state through the effect of the temperature field, causes collision and friction between the quartz sands through the effect of the ultrasonic field and further increases the internal activation energy, further increases the internal energy of the gas-liquid inclusions through the effect of the infrared light field, and then promotes the quartz sand containing the gas-liquid inclusions to burst from the inside through the instantaneous excitation of the quartz sand by the laser field, and further bursts the high-temperature quartz sand through cold quenching. The multi-field coupling auxiliary effect and cold quenching effect increase the probability of quartz sand particle bursting, causing the gas-liquid inclusions to overflow from the quartz sand, thereby achieving deep removal.

[0021] The components of the alkaline washing liquid and the pickling liquid used in the present invention include deionized water, anhydrous sodium carbonate, guanidine carbonate, disodium ethylenediaminetetraacetic acid, malic acid, citric acid and polyethylene, all of which are green and environmentally friendly chemical reagents. Deionized water is pure and free of impurities and is used as a solvent. Anhydrous sodium carbonate and guanidine carbonate are alkaline reagents used to soften, loosen and disperse impurities and silicate substances attached to the surface of quartz sand. Disodium ethylenediaminetetraacetic acid is used as a surfactant to increase the activity of chemical reagents and enhance the alkaline washing effect. Malic acid and citric acid are acidic reagents used to remove oxides and various ionic impurities on the surface of quartz sand. Polyethylene is used as a wetting agent to increase the wetting effect of the pickling liquid on the surface of quartz sand, so that the pickling liquid can enter the gaps on the surface of quartz sand and enhance the cleaning effect.

[0022] During the cleaning process, the present invention controls the temperature field, utilizes the flow field assistance generated by ultrasonic assistance and stirring, and cooperates with the chemical action of alkaline cleaning solution and acid cleaning solution to form an impurity removal mechanism of chemical and multi-field assistance coupling, thereby effectively achieving the deep removal of gas-liquid inclusions wrapped by quartz sand impurities.

[0023] The present invention has the following advantages:

[0024] 1. Through the synergistic effect of temperature field, ultrasonic field, infrared light field and laser field, as well as cold quenching, the probability of quartz sand particles containing gas-liquid inclusions bursting from the inside is greatly increased, allowing the gas-liquid inclusions to overflow and achieve deep removal.

[0025] 2. Both alkaline cleaning solution and acid cleaning solution are green and environmentally friendly solutions. They do not contain strong acids, strong alkalis and toxic substances, and will not cause significant harm to the human body and the environment. They are in line with the current green manufacturing concept.

[0026] 3. Before alkaline washing and acid washing, make full use of multi-energy field assistance and cold quenching to make the quartz sand burst or create gaps. During cleaning, use the flow field assistance generated by temperature field, ultrasonic field and stirring to form a coupling effect with the chemical field, which can deeply remove impurities including gas-liquid inclusions and improve the efficiency of impurity removal. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0028] Figure 1 It is a front view of the overall structure of the equipment used in the embodiment of the present invention.

[0029] Figure 2 This is a schematic diagram of the three-dimensional structure of the multi-field coupling assisted high-purity quartz sand impurity deep removal equipment in an embodiment of the present invention.

[0030] Figure 3 It is a schematic diagram of the three-dimensional structure of the charging bin used in the embodiment of the present invention.

[0031] Figure 4 Schematic diagram of the laser and infrared light system used in the embodiment of the present invention.

[0032] Figure 5 Surface state of a quartz crucible 1 made of quartz sand melted without using the present invention to remove impurities.

[0033] Figure 6 Surface state of a quartz crucible 2 made of quartz sand without removing impurities according to the present invention.

[0034] Figure 7 Surface state of a quartz crucible 3 made of quartz sand melted without using the present invention to remove impurities.

[0035] Figure 8 The surface state of the quartz crucible 4 made by melting the quartz sand after removing impurities according to the present invention.

[0036] Fig. 9 The surface state of the quartz crucible 5 made by melting quartz sand after removing impurities according to the present invention.

[0037] Fig.10 The surface state of the quartz crucible 6 made by melting quartz sand after removing impurities according to the present invention.

[0038] In the figure: 1. Frame; 2. Workbench mechanism, 3. Ultrasonic vibration table, 4. Loading mechanism, 5. Control system, 6. Laser and infrared light system, 7. Rotating and telescopic spindle, 8. Temperature control system, 9. Cold quenching and cleaning mechanism;

[0039] Among them, 1-1. workbench track, 1-2. processing cabin, 1-3. horizontal partition, 1-4. electronic component cabin, 1-5 electronic component cabin door, 1-6. inner window, 1-7. processing cabin door; 2-1. workbench motor, 2-2. workbench, 2-3. hinge; 3-1. ultrasonic vibrator, 3-2. ultrasonic concentrator; 4-1. loading bin door, 4-2. bin door track, 4-3. loading bin; 6-1 infrared light generator, 6-2. weak laser generator, 6-3. optical path system, 6-4 strong laser generator; 7-1. spindle rotation motor, 7-2. reduction gear set, 7-3 hydraulic mechanism, 7-4 hydraulic gear set, 7-5. hydraulic motor; 9-1 cold quenching cleaning cabin, 9-2 cabin cover, 9-3 impeller, 9-4 cabin cover. DETAILED DESCRIPTION

[0040] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0041] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0043] Unless otherwise specifically stated, the relative arrangement of the parts and steps described in these embodiments, the numerical expressions and numerical values ​​do not limit the scope of the present invention. At the same time, it should be clear that, for ease of description, the sizes of the various parts shown in the drawings are not drawn according to the actual proportional relationship. The technology, methods and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be regarded as part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar numbers and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further discussed in subsequent drawings.

[0044] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings. They are only for the convenience of describing the present invention and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of the present invention: the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.

[0045] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below their position devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0046] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0047] The embodiment of the present invention discloses a method for deep removal of impurities in high-purity quartz sand assisted by multi-energy field coupling, which is implemented based on the following device:

[0048] like Figure 1-4 As shown, a multi-field synergistically assisted high-purity quartz sand gas-liquid inclusion deep removal equipment, by using ultrasonic field, temperature field, laser field and infrared light field multi-field synergistically assisted to deeply remove gas-liquid inclusions in quartz sand, fundamentally achieving the goal of high-quality and high-efficiency deep removal of gas-liquid inclusions in high-purity quartz sand.

[0049] Specifically, it includes a frame 1, a workbench mechanism 2, an ultrasonic vibration table 3, a loading mechanism 4, a control system 5, a laser and infrared light system 6, a rotating telescopic main shaft 7 and a temperature control system 8. The workbench 2-2 is installed at the bottom of the frame 1, and the ultrasonic vibration table 3 is connected to the workbench 2-2 through a hinge 2-3 and a hydraulic rod. The loading bin 4-2 is set on the ultrasonic vibration table 3, the operating system 5 is installed on one side of the frame 1, the laser and infrared system 6 is fixed at the end of the rotating telescopic main shaft 7, and there is a preset distance between the bottom of the laser and infrared system 6 and the top of the loading mechanism 4. The rotating telescopic main shaft 7 is installed above the equipment processing cabin 1-2 through a horizontal partition 1-2, and the temperature control system 8 is set on both sides and the rear side of the processing cabin 1-2.

[0050] The frame 1 includes a shell, a workbench track 1-1, a processing cabin 1-2, a horizontal partition 1-3, an electronic component cabin 1-4 and its door 1-5, an inner window 1-6, and a processing cabin door 1-7. The shell is a rectangular parallelepiped, which is divided into a processing cabin 1-2 and an electronic component cabin 1-4 by a horizontal partition 1-3. The electronic component cabin 1-4 is installed with electronic components of the equipment and a spindle rotating motor 7-1 and a hydraulic motor 7-5, a hydraulic mechanism 7-3, etc. of the rotating and telescopic spindle 7 above. The processing cabin 1-2 is installed with a workbench mechanism 2, an ultrasonic vibration table 3, a loading mechanism 4, a laser and infrared system 6, a rotating and telescopic spindle 7, and a temperature control system 8.

[0051] The workbench mechanism 2 includes a motor 2-1, a workbench 2-2, a hinge 2-3 and a hydraulic telescopic rod. The motor 2-1 is arranged on the frame 1 below the workbench 2-2, the workbench 2-2 is cylindrical, the hinge 2-3 is installed on the front side of the workbench 2-2, connecting the workbench 2-2 and the ultrasonic vibration table 3, and the hydraulic telescopic rod is arranged inside the workbench 2-2, the input end of the hydraulic telescopic rod is connected to the motor 2-1, and the output end is connected to the ultrasonic vibration table 3. Driven by the motor 2-1, the hydraulic telescopic rod can lift the ultrasonic vibration table 3 from the rear side.

[0052] The ultrasonic vibration table 3 includes an ultrasonic vibrator 3-1 and an ultrasonic concentrator 3-2, wherein 8 ultrasonic vibrators 3-1 are arranged evenly inside the ultrasonic vibration table 3, which can realize ultrasonic vibration of the upper loading bin 4-2, increase the activation energy of the gas-liquid inclusions in the quartz sand and make the quartz sand rub and collide with each other.

[0053] The loading mechanism 4 includes a loading bin 4-3, a bin door 4-1 and a bin door track 4-2. The bin door 4-1 is arranged in front of the loading bin 4-3, and the bin door track 4-2 is arranged on one side of the bin door 4-1. The loading bin 4-3 is used as a processing container for quartz sand. When the bin door 4-1 is opened, one side of the loading bin mechanism is lifted by the hydraulic telescopic rod in the workbench mechanism 2 to pour out the processed quartz sand.

[0054] The operating system 5 includes switches and an operating panel, which can realize the operation of the workbench mechanism 2, the ultrasonic vibration table 3, the loading mechanism 4, the laser and infrared system 5, the rotating and telescopic main shaft 6 and the temperature control system 7.

[0055] The laser and infrared system 6 includes an infrared generator 6-1, a weak laser generator 6-2, a strong laser generator 6-4 and an optical path system 6-3, wherein the infrared generator 6-1 is set in a group, and the laser sets the weak laser generator 6-2 and the strong laser generator 6-4 according to the intensity, and the laser intensity can be adjusted within a range. Infrared light assistance can achieve a moderate increase in the molecular internal energy in quartz sand, and laser assistance can instantly increase the molecular internal energy and activation energy in quartz sand, so as to achieve particle cracking or even explosion, thereby causing the gas-liquid inclusion to overflow.

[0056] The rotating telescopic main shaft 7 includes a rotating control motor 7-1, a reduction gear set 7-2, a hydraulic pump motor 7-5, a hydraulic mechanism 7-3 and a hydraulic gear set 7-4. Each component is arranged inside the electronic component compartment 1-4 above the horizontal partition 1-3. The rotating control motor 7-1 controls the rotation of the main shaft through the reduction gear set 7-2, and the hydraulic motor 7-5 controls the extension and retraction of the main shaft through the hydraulic gear set 7-4 and the hydraulic mechanism 7-3. Turning on the rotating motor 7-1 can make the main shaft rotate and drive the laser and infrared system 6 to rotate, so that the infrared light and lasers of different intensities can be uniformly irradiated on the quartz sand. Starting the hydraulic pump motor 7-5 can adjust the extension and retraction length of the main shaft, thereby adjusting the illumination distance.

[0057] The temperature control system 8 can enable the quartz sand to maintain a high energy state.

[0058] It also includes a cold extraction cleaning mechanism, which includes a shell 9-1, a cold extraction cleaning chamber 9-2, an impeller 9-3, and a chamber cover 9-4. A motor, an ultrasonic vibration device, and a temperature control device are arranged inside the shell. Through the stirring of the impeller 9-3 and the assistance of ultrasound and temperature, the quartz sand can be fully cold-quenched and deeply cleaned in all directions under the ultrasonic field, temperature field, and stirring flow field coupled chemical field.

[0059] In summary, the multi-energy field synergistically assisted high-purity quartz sand gas-liquid inclusion deep removal equipment provided by the present invention maintains the quartz sand in a high energy state through the action of the temperature field, generates collision friction between the quartz sands through the action of the ultrasonic field and further increases the internal activation energy, further increases the internal energy of the gas-liquid inclusions through the action of the infrared light field, and then promotes the quartz sand containing gas-liquid inclusions to explode from the inside by instantaneously exciting the quartz sand through the laser field. The synergistic effect of multiple fields increases the efficiency of the quartz sand particle explosion, making it easier for gas-liquid inclusions to overflow from the quartz sand, fundamentally achieving the goal of high-quality and efficient deep removal of gas-liquid inclusions in high-purity quartz sand.

[0060] The specific application method of the present invention is as follows: Step 1, placing the quartz sand to be processed in the loading bin, closing the processing cabin door, turning on the temperature control system, setting the processing cabin temperature to 400-800° C., and preheating the quartz sand;

[0061] Step 2, set the ultrasonic vibration frequency to 50-100kHz, set the infrared light output, set the weak laser output intensity to 0-10mW and the strong laser output intensity to 30-80mW respectively, set the rotation and telescopic spindle parameters, determine the rotation speed of the laser and infrared system to 0-10r / min and the distance from the quartz sand to 20-100cm, set the processing time to 3-6 hours, and start the first stage of processing;

[0062] Step 3: Add 2 / 5 to 3 / 5 volume of deionized water to the cold quench cleaning mechanism, set the temperature to 0 to 5°C, cool the deionized water to 0 to 5°C, and maintain it;

[0063] After step 4 and step 2 are completed, open the hatch of the processing cabin, transport the processing platform along the track to the cold extraction cleaning mechanism, open the hatch of the loading bin, open the hydraulic telescopic mechanism in the processing platform, pour the quartz sand into the cold extraction cleaning cabin for cold extraction for 30 to 60 minutes. At the same time, set the ultrasonic frequency of the cold quenching cleaning mechanism to 20 to 200kHz, the stirring speed to 20 to 80r / min, and start stirring the cold extraction;

[0064] Step 5: After the cold extraction is completed, the quartz sand is taken out, and the deionized water in the cleaning chamber is replaced with a green alkaline cleaning solution, wherein the alkaline cleaning solution is non-toxic, harmless, green and environmentally friendly, and the ingredients include: deionized water, anhydrous sodium carbonate 50-100g / L, guanidine carbonate 20-80g / L, and disodium ethylenediaminetetraacetate 5-15vol.%. The temperature is set to 200-400℃, the ultrasonic frequency is set to 20-200kHz, the stirring speed is set to 20-80r / min, and the alkaline cleaning is started for 5-8 hours;

[0065] Step 6: After the alkaline washing is completed, the quartz sand is taken out and the alkaline washing liquid in the washing chamber is replaced with a green and environmentally friendly acid washing liquid, wherein the acid washing liquid is non-toxic and harmless, green and environmentally friendly, and the ingredients include: deionized water, malic acid 100-200g / L, citric acid 80-150g / L, polyethylene 5-10vol.%. Set the temperature to 200-400℃, set the ultrasonic frequency to 20-200kHz, set the stirring speed to 20-80r / min, and start acid washing for 5-10 hours;

[0066] Step 7: After pickling, take out the quartz sand, replace the pickling liquid in the cleaning chamber with anhydrous ethanol, set the temperature to 20-30°C, set the ultrasonic frequency to 20-200kHz, set the stirring speed to 20-80r / min, and start cleaning for 30-60min;

[0067] Step 8: After cleaning, use an air dryer to dry the product at a temperature of 30 to 50°C.

[0068] The present invention keeps the quartz sand in a high energy state through the effect of the temperature field, causes collision and friction between the quartz sands through the effect of the ultrasonic field and further increases the internal activation energy, further increases the internal energy of the gas-liquid inclusions through the effect of the infrared light field, and then promotes the quartz sand containing the gas-liquid inclusions to burst from the inside through the instantaneous excitation of the quartz sand by the laser field, and further bursts the high-temperature quartz sand through cold quenching. The multi-field coupling auxiliary effect and cold quenching effect increase the probability of quartz sand particle bursting, causing the gas-liquid inclusions to overflow from the quartz sand, thereby achieving deep removal.

[0069] The components of the alkaline washing liquid and the pickling liquid used in the present invention include deionized water, anhydrous sodium carbonate, guanidine carbonate, disodium ethylenediaminetetraacetic acid, malic acid, citric acid and polyethylene, all of which are green and environmentally friendly chemical reagents. Deionized water is pure and free of impurities and is used as a solvent. Anhydrous sodium carbonate and guanidine carbonate are alkaline reagents used to soften, loosen and disperse impurities and silicate substances attached to the surface of quartz sand. Disodium ethylenediaminetetraacetic acid is used as a surfactant to increase the activity of chemical reagents and enhance the alkaline washing effect. Malic acid and citric acid are acidic reagents used to remove oxides and various ionic impurities on the surface of quartz sand. Polyethylene is used as a wetting agent to increase the wetting effect of the pickling liquid on the surface of quartz sand, so that the pickling liquid can enter the gaps on the surface of quartz sand and enhance the cleaning effect.

[0070] During the cleaning process, the present invention controls the temperature field, utilizes the flow field assistance generated by ultrasonic assistance and stirring, and cooperates with the chemical action of alkaline cleaning solution and acid cleaning solution to form an impurity removal mechanism of chemical and multi-field assistance coupling, thereby effectively achieving the deep removal of gas-liquid inclusions wrapped by quartz sand impurities.

[0071] The specific operations are as follows

[0072] Example 1

[0073] Step 1: Place the quartz sand to be processed in the loading bin 4-2, close the processing chamber door 4-3, turn on the temperature control system 8, set the processing chamber temperature to 800°C, and preheat the quartz sand;

[0074] Step 2, set the ultrasonic vibration frequency to 50kHz, set the infrared output parameters, set the weak laser output intensity to 2mW and the strong laser output intensity to 50mW respectively, set the parameters of the rotating telescopic spindle 7, determine the rotation speed of the laser and infrared system 6 to 1r / min and the distance from the quartz sand to 20cm, set the processing time to 4 hours, and start the first stage of processing;

[0075] Step 3: Add 3 / 5 volume of deionized water to the cold quench cleaning mechanism 9, set the temperature to 5°C, cool the deionized water to 5°C, and maintain it.

[0076] After step 4 and step 2 are completed, open the processing cabin door 1-7, transport the processing platform 2-2 along the track to the cold extraction cleaning mechanism 9, open the loading bin door 4-2, open the hydraulic telescopic mechanism in the processing platform 2-2, pour the quartz sand into the cold extraction cleaning cabin 9-2 for cold extraction for 60 minutes. At the same time, set the ultrasonic frequency of the cleaning mechanism to 100kHz, set the stirring speed to 30r / min, and start stirring the cold extraction;

[0077] Step 5. After the cold extraction is completed, the quartz sand is taken out, and the deionized water in the cleaning chamber 9-2 is replaced with a green alkaline cleaning solution, wherein the alkaline cleaning solution is non-toxic and harmless, green and environmentally friendly, and its ingredients include: deionized water, anhydrous sodium carbonate 50g / L, guanidine carbonate 20g / L, and disodium ethylenediaminetetraacetate 5vol.%. The temperature is set to 200°C, the ultrasonic frequency of the cleaning mechanism is set to 100kHz, the stirring speed is set to 30r / min, and the alkaline cleaning is started for 6 hours;

[0078] Step 6: After the alkaline washing is completed, the quartz sand is taken out, and the alkaline washing liquid in the washing chamber 9-2 is replaced with a green and environmentally friendly acid washing liquid, wherein the acid washing liquid is non-toxic and harmless, green and environmentally friendly, and its ingredients include: deionized water, malic acid 100g / L, citric acid 80g / L, polyethylene 5vol.%. Set the temperature to 200℃, set the ultrasonic frequency to 100kHz, set the stirring speed to 30r / min, and start acid washing for 6 hours;

[0079] Step 7: After pickling, take out the quartz sand, replace the pickling liquid in the cleaning chamber 9-2 with anhydrous ethanol, set the temperature to 20°C, set the ultrasonic frequency to 100kHz, set the stirring speed to 30r / min, and start cleaning for 30min;

[0080] Step 8: After cleaning, use an air dryer to dry the product at a temperature of 30°C.

[0081] Example 2

[0082] Step 1: Place the quartz sand to be processed in the loading bin 4-2, close the processing chamber door 4-3, turn on the temperature control system 8, set the processing chamber temperature to 600°C, and preheat the quartz sand;

[0083] Step 2, set the ultrasonic vibration frequency to 60kHz, set the infrared output parameters, set the weak laser output intensity to 5mW and the strong laser output intensity to 80mW respectively, set the parameters of the rotating telescopic spindle 7, determine the rotation speed of the laser and infrared system 6 to 2r / min and the distance from the quartz sand to 50cm, set the processing time to 5 hours, and start the first stage of processing;

[0084] Step 3: Add 3 / 5 volume of deionized water to the cold quench cleaning mechanism 9, set the temperature to 3°C, cool the deionized water to 3°C, and maintain it.

[0085] After step 4 and step 2 are completed, open the processing cabin door 1-7, transport the processing platform 2-2 along the track to the cold extraction cleaning mechanism 9, open the loading bin door 4-2, open the hydraulic telescopic mechanism in the processing platform 2-2, pour the quartz sand into the cold extraction cleaning cabin 9-2 for cold extraction for 50 minutes. At the same time, set the ultrasonic frequency of the cleaning mechanism to 80kHz, set the stirring speed to 50r / min, and start stirring the cold extraction;

[0086] Step 5. After the cold extraction is completed, the quartz sand is taken out, and the deionized water in the cleaning chamber 9-2 is replaced with a green alkaline cleaning solution, wherein the alkaline cleaning solution is non-toxic and harmless, green and environmentally friendly, and its ingredients include: deionized water, anhydrous sodium carbonate 70g / L, guanidine carbonate 40g / L, and disodium ethylenediaminetetraacetate 7vol.%. The temperature is set to 280°C, the ultrasonic frequency of the cleaning mechanism is set to 80kHz, the stirring speed is set to 50r / min, and the alkaline cleaning is started for 8 hours;

[0087] Step 6: After the alkaline washing is completed, the quartz sand is taken out, and the alkaline washing liquid in the washing chamber 9-2 is replaced with a green and environmentally friendly acid washing liquid, wherein the acid washing liquid is non-toxic and harmless, green and environmentally friendly, and its ingredients include: deionized water, malic acid 120g / L, citric acid 100g / L, polyethylene 8vol.%. Set the temperature to 280℃, set the ultrasonic frequency to 80kHz, set the stirring speed to 50r / min, and start acid washing for 8 hours;

[0088] Step 7: After pickling, take out the quartz sand, replace the pickling liquid in the cleaning chamber 9-2 with anhydrous ethanol, set the temperature to 25°C, set the ultrasonic frequency to 80kHz, set the stirring speed to 40r / min, and start cleaning for 40min;

[0089] Step 8: After cleaning, use an air dryer to dry the product at a temperature of 40°C.

[0090] Example 3

[0091] Step 1: Place the quartz sand to be processed in the loading bin 4-2, close the processing chamber door 4-3, turn on the temperature control system 8, set the processing chamber temperature to 600°C, and preheat the quartz sand;

[0092] Step 2, set the ultrasonic vibration frequency to 100kHz, set the infrared output parameters, set the weak laser output intensity to 5mW and the strong laser output intensity to 60mW respectively, set the parameters of the rotating telescopic spindle 7, determine the rotation speed of the laser and infrared system 6 to 1r / min and the distance from the quartz sand to 60cm, set the processing time to 6 hours, and start the first stage of processing;

[0093] Step 3: Add 2 / 5 volume of deionized water to the cold quench cleaning mechanism 9, set the temperature to 1°C, cool the deionized water to 1°C, and maintain it.

[0094] After step 4 and step 2 are completed, open the processing cabin door 1-7, transport the processing platform 2-2 along the track to the cold extraction cleaning mechanism 9, open the loading bin door 4-2, open the hydraulic telescopic mechanism in the processing platform 2-2, pour the quartz sand into the cold extraction cleaning cabin 9-2 for cold extraction for 40 minutes. At the same time, set the ultrasonic frequency of the cleaning mechanism to 120kHz, set the stirring speed to 50r / min, and start stirring the cold extraction;

[0095] Step 5. After the cold extraction is completed, the quartz sand is taken out, and the deionized water in the cleaning chamber 9-2 is replaced with a green alkaline cleaning solution, wherein the alkaline cleaning solution is non-toxic and harmless, green and environmentally friendly, and its ingredients include: deionized water, anhydrous sodium carbonate 60g / L, guanidine carbonate 80g / L, and disodium ethylenediaminetetraacetate 10vol.%. The temperature is set to 300°C, the ultrasonic frequency of the cleaning mechanism is set to 120kHz, the stirring speed is set to 50r / min, and the alkaline cleaning is started for 7 hours;

[0096] Step 6: After the alkaline washing is completed, the quartz sand is taken out, and the alkaline washing liquid in the washing chamber 9-2 is replaced with a green and environmentally friendly acid washing liquid, wherein the acid washing liquid is non-toxic and harmless, green and environmentally friendly, and its ingredients include: deionized water, malic acid 100g / L, citric acid 150g / L, polyethylene 10vol.%. Set the temperature to 300℃, set the ultrasonic frequency to 120kHz, set the stirring speed to 50r / min, and start acid washing for 8 hours;

[0097] Step 7: After pickling, take out the quartz sand, replace the pickling liquid in the cleaning chamber 9-2 with anhydrous ethanol, set the temperature to 30°C, set the ultrasonic frequency to 120kHz, set the stirring speed to 50r / min, and start cleaning for 50min;

[0098] Step 8: After cleaning, use an air dryer to dry the product at a temperature of 50°C.

[0099] The multi-energy field coupling assisted high-purity quartz sand impurity deep removal method provided by the present invention maintains the quartz sand in a high energy state through the action of the temperature field, generates collision friction between the quartz sands through the action of the ultrasonic field and further increases the internal activation energy, further increases the internal energy of the gas-liquid inclusions through the action of the infrared light field, promotes the quartz sand containing gas-liquid inclusions to burst from the inside through the instantaneous excitation of the quartz sand by the laser field, and further bursts the high-temperature quartz sand through cold quenching. The multi-field coupling assisted action and cold quenching action increase the probability of quartz sand particle bursting, causing gas-liquid inclusions to overflow therefrom. Combined with the temperature field, and using the flow field assisted by ultrasonic assistance and stirring, the quartz sand is alkali-washed and acid-washed respectively, forming a multi-field assisted and chemical field coupled cleaning, and removing impurities including gas-liquid inclusions from a deep level and efficiently.

[0100] Example Product Application: Impurities in high-purity quartz sand have a great impact on the quality of melting high-purity quartz crucibles. In order to verify the effect of removing impurities in quartz sand by the present invention, three batches of high-purity quartz sand were selected to directly melt quartz crucibles and to melt quartz crucibles after removing impurities using the three embodiments of the present invention, and their quality effects were compared. The results are as follows:

[0101] Table 1 Quartz crucible made of high-purity quartz sand melted without removing impurities using the present invention

[0102] serial number Number of surface defects <![CDATA[Bubble density (number / cm 2 ) <!-- 8 -->]]> 1 13 56 2 9 78 3 8 37

[0103] Table 2 Quartz crucible melted by high-purity quartz sand after impurities are removed by the present invention

[0104] serial number Number of surface defects <![CDATA[Bubble density (pcs / cm 2 )]]> 4 2 8 5 1 11 6 1 5

[0105] The surfaces of the melted quartz crucibles were observed using a microscope. The surface conditions of the quartz crucibles No. 1 to 3 melted from the high-purity quartz sand without removing impurities using the present invention correspond to the surface conditions of the quartz crucible No. 1 to 3 melted from the high-purity quartz sand without removing impurities using the present invention. Figure 5-7 The surface state of the quartz crucible No. 4-6 made by melting the high-purity quartz sand after removing impurities according to the present invention corresponds to the surface state of the quartz crucible No. 4-6 made by melting the high-purity quartz sand after removing impurities according to the present invention. Figure 8-10It can be clearly seen that compared with the quartz crucible made of quartz sand without removing impurities by the present invention, the surface quality of the quartz crucible made of quartz sand after removing impurities by the present invention is significantly improved, not only the number of bubbles is reduced, but also the size of the bubbles is reduced.

[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A multi-energy field coupling assisted high-purity quartz sand impurity deep removal method, characterized in that: The specific steps are as follows: Step 1, preheating the quartz sand at 400-800°C; Step 2, the preheated quartz sand is processed by ultrasonic vibration, laser and infrared synchronously, and the processing time is 3 to 6 hours; Step 3, cold quenching and cleaning the quartz sand processed in step 2; Step 4, alkali washing and acid washing are respectively performed on the quartz sand after cold quenching and cleaning; Step 5: The quartz sand treated in step 4 is cleaned by ultrasonic stirring with anhydrous ethanol, and then dried after cleaning.

2. A multi-energy field coupling assisted high-purity quartz sand impurity deep removal method according to claim 1, characterized in that: In step 2, the ultrasonic vibration frequency is set to 50-100 kHz.

3. The multi-energy field coupling-assisted high-purity quartz sand impurity deep removal method according to claim 1 is characterized in that: In step 3, add 3 / 5 volume of deionized water to the cold quenching cleaning mechanism, set the temperature to 0-5°C, cool the deionized water to 0-5°C, and maintain it; after completing step 2, transport the quartz sand to the cold extraction cleaning mechanism, pour the quartz sand into the cold extraction cleaning cabin for cold extraction for 30-60 minutes, and at the same time set the ultrasonic frequency of the cold quenching cleaning mechanism to 20-200kHz, the stirring speed to 20-80r / min, and start stirring the cold extraction.

4. The method for deep removal of impurities from high-purity quartz sand assisted by multi-energy field coupling according to claim 1 is characterized in that: In step 4, after the cold extraction is completed, the quartz sand is taken out, and the deionized water in the cleaning chamber is replaced with a green and environmentally friendly alkaline washing solution. During the alkaline washing process, the temperature is set at 200-400°C, the ultrasonic frequency is set at 20-200kHz, the stirring speed is set at 20-80r / min, and the alkaline washing is started for 5-8 hours.

5. The method for deep removal of impurities from high-purity quartz sand assisted by multi-energy field coupling according to claim 1 is characterized in that: The composition of the alkaline washing solution is in units of mass concentration, and includes the following components in concentrations: 50-100 g / L of anhydrous sodium carbonate, 20-80 g / L of guanidine carbonate, and 5-15 vol.% of disodium ethylenediaminetetraacetate.

6. The multi-energy field coupling-assisted high-purity quartz sand impurity deep removal method according to claim 1 is characterized in that: In step 4, after the alkaline washing is completed, the quartz sand is taken out, and the alkaline washing liquid in the cleaning chamber is replaced with a green and environmentally friendly acid washing liquid. During the acid washing process, the temperature is set at 200-400°C, the ultrasonic frequency is set at 20-200kHz, the stirring speed is set at 20-80r / min, and the acid washing is started for 5-10 hours.

7. According to claim 1, the multi-energy field coupling assisted high-purity quartz sand impurity deep removal method is characterized in that: The pickling liquid composition is in units of mass concentration, and includes components of the following concentrations: malic acid 100-200 g / L, citric acid 80-150 g / L, polyethylene 5-10 vol.%.

8. The multi-energy field coupling-assisted high-purity quartz sand impurity deep removal method according to claim 1 is characterized in that: In step 5, after the pickling is completed, the quartz sand is taken out, the pickling liquid in the cleaning chamber is replaced with anhydrous ethanol, the temperature is set to 20-30°C, the ultrasonic frequency is set to 20-200kHz, the stirring speed is set to 20-80r / min, and the cleaning is started for 30-60min; After cleaning, use a blower dryer to dry at a temperature of 30 to 50°C.

Citation Information

Patent Citations

  • Preparation method of highly pure quartz sands

    CN105948062A

  • Method for purifying quartz sand

    CN108033454A

  • Method for purifying quartz sands by microwave-vacuum combined roasting

    CN112010317A

  • Ceramic raw material impurity removal and purification device and use method thereof

    CN116673208A

  • Quartz sand purification method and quartz sand laser purification device

    CN117720110A

Cited By

  • Deep removal method for lattice impurities and inclusions in high-purity quartz sand

    CN120423562A