Method for preparing activated zeolite without harmful heavy metals
Through alkali modification and multi-step treatment technology, harmful heavy metals in natural zeolites have been successfully removed, solving the problems of aluminum dissolution and adsorption of beneficial elements under gastric acid conditions, and improving the quality of feed and cosmetics.
Patent Information
- Application Number
- CN202410525746.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-02-20
- Filing Date
- 2024-04-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-29
AI Technical Summary
The prior art is difficult to effectively remove harmful heavy metals in natural zeolites, such as arsenic, lead, mercury, and cadmium. Especially the problems of aluminum dissolution and adsorption and excretion of beneficial elements under gastric acid conditions, which affects the quality of feed and cosmetics.
By modifying and unblocking natural zeolites, combining the treatment of phosphoric acid, ferrous salt, hydroxylamine hydrochloride and complexing agent, adjust the pH value and ionic strength, and use oxidant precipitation and stand-alone natural precipitation technology to gradually separate and deposit harmful heavy metals. Finally, Active zeolites without harmful heavy metals were obtained through high temperature activation.
It significantly reduces the content of harmful heavy metals in natural zeolites, improves the quality of feed and cosmetics, and ensures the reduction of aluminum dissolution under gastric acid conditions and maintains hemostatic properties.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of zeolite treatment methods, in particular to a method for manufacturing activated zeolite without harmful heavy metals. Background Art
[0002] According to incomplete statistics, my country has discovered nearly 400 natural zeolite deposits with a total reserve of about 3 billion tons. There are many types of natural zeolites. There are more than 80 different types of zeolites in nature. Different types of zeolites have different characteristics and applications. Natural zeolites are acid-resistant and alkali-resistant, and have excellent stability, ion exchange, hemostatic properties and the ability to adsorb harmful substances. Natural zeolites are widely used in sewage treatment, soil improvement, air purification, ion exchange materials, catalysts, animal feed, cosmetics, medical devices and other fields.
[0003] As a feed additive, zeolite can increase the activity of some enzymes in animals, improve antioxidant capacity, reduce harmful substances such as aflatoxin and heavy metals in the body, reduce the body's nitrate burden, and reduce ammonia in feces, which is beneficial to colon microbiota and epithelial cells. In addition, zeolite also has "nutritional" value. Adding 5% zeolite powder to feed can accelerate the growth of poultry and livestock, make them strong and fresh, and increase egg production. Zeolite is acid-resistant and alkali-resistant, has excellent stability and ion exchange, hemostatic properties, and the ability to adsorb harmful substances. When added to feed and entering the gastrointestinal tract of animals, harmful heavy metals such as lead, mercury, and cadmium, and radioactive elements such as cesium, radium, and strontium will be captured and fixed in the zeolite pore structure and excreted from the body with excrement. Adding it to feed is conducive to eliminating harmful heavy metals in the gastrointestinal tract of animals, making animals healthier. However, zeolite without modification will dissolve aluminum under gastric acid conditions, which will increase the aluminum intake of animals and have an adverse effect; the excellent ion exchange performance of zeolite will even adsorb and excrete beneficial elements (such as calcium, iron, and zinc) in animals, making the daily intake of beneficial elements required by animals insufficient and affecting animal health. At present, my country's feed hygiene standards only stipulate the judgment value of arsenic in zeolite, and other harmful heavy metals are not specified. Zeolite as a feed additive does not specify the judgment value of harmful heavy metals (lead, mercury, cadmium, etc.), which may lead to high levels of other harmful heavy metals in feed and affect its quality. In addition, zeolite is added as a raw material in cosmetics, which can effectively absorb many harmful substances in human skin and has excellent skin cleansing effect and is widely used. According to the requirements of my country's "Technical Specifications for Safety of Cosmetics", the relevant limit standards for harmful heavy metals in cosmetics are lead ≤10mg / kg, mercury ≤1mg / kg, arsenic ≤2mg / kg, and cadmium ≤5mg / kg. However, there is no specified determination value for harmful heavy metals (lead, arsenic, mercury, cadmium) in zeolite as a raw material for cosmetics. If the harmful heavy metal content of zeolite as a raw material is high, it will lead to high harmful heavy metal content in cosmetics, which will also affect its quality. As people's living standards improve, the limit of harmful substance content of zeolite as a feed additive and cosmetic raw material will gradually increase. Therefore, inventing a technology to remove harmful heavy metals in zeolite has great social value.
[0007] Many early studies were based on the use of zeolites to treat (adsorb) sewage or soil contaminated by heavy metals. Some literature reported the use of complexing agents or chelating agents to remove soil contaminated by heavy metals through leaching methods; and a small number of literature reported the removal of arsenic from wastewater by modified zeolites. No literature reported methods for completely removing harmful heavy metals such as lead, arsenic, mercury, and cadmium from natural zeolites, solving the problem of aluminum dissolution in zeolites under gastric acid conditions, and inhibiting or reducing the adsorption and excretion of beneficial elements (such as calcium, iron, and zinc) from the body.
[0008] Zeolite is a kind of aluminosilicate. The composition of natural zeolite is complex. A large number of studies have shown that the content of harmful heavy metals such as lead, arsenic, mercury and cadmium is high. The content of some harmful heavy metals such as lead and arsenic can reach or exceed 15 mg / kg. Natural zeolite is added to feed and cosmetics without treatment, which makes the content of heavy metals in cosmetics and feed high. There are many ion dissolution and ion exchange in the solution system of natural zeolite. Therefore, there are inevitably many ion exchanges and ion dissolution in the solution system of natural zeolite. Harmful heavy metals such as lead, mercury and cadmium in natural zeolite are cations. The valence state of arsenic is relatively complex. Generally speaking, the harmful heavy metal arsenic in natural zeolite is similar to arsenic in soil. The harmful heavy metal arsenic is mainly trivalent arsenic and pentavalent arsenic; the arsenic forms in natural zeolite include water-soluble arsenic, weakly adsorbed arsenic, strongly adsorbed arsenic, amorphous iron-aluminum oxide-bound arsenic, crystalline iron-aluminum oxide-bound arsenic, and calcium-bound arsenic. Except for water-soluble arsenic and weakly adsorbed arsenic, other bound arsenic is difficult to be physically separated from natural zeolite. Natural zeolite contains a certain amount of iron (or ferrous iron) and calcium. Therefore, calcium ions and iron (or ferrous iron) ions are dissolved in the natural zeolite solution system. Oxygen is inevitably present in the solution system. The ferrous iron dissolved in the natural zeolite within a wide pH range of the solution system is very easily oxidized into iron ions (combined with the iron ions dissolved in the natural zeolite) and the dissolved harmful heavy metal arsenate ions (or arsenite ions) continue to form insoluble precipitates. Therefore, the harmful heavy metal arsenic cannot be effectively physically separated from the natural zeolite. The complex composition of natural zeolite and the easy formation of insoluble arsenic make it very difficult to remove arsenic from natural zeolite. Therefore, it is very difficult to remove harmful heavy metals in natural zeolite, which poses a huge challenge.
[0009] Natural zeolite contains high levels of silicon and aluminum, so there is obvious aluminum dissolution under animal gastric acid conditions. Therefore, it is extremely challenging and difficult to prepare harmful heavy metal-free zeolite with low aluminum dissolution under simulated gastric acid conditions, strong adsorption of harmful heavy metals, and excellent hemostatic properties. It also has important social significance. Summary of the invention
[0010] 1. Technical issues to be resolved
[0011] In view of the shortcomings of the prior art, the present invention provides a method for manufacturing activated zeolite without harmful heavy metals, so as to solve the problems raised in the above background technology, such as it is very difficult to remove arsenic from natural zeolite, it is difficult to remove harmful heavy metals exceeding the standard in natural zeolite, and it is extremely challenging and difficult to prepare harmful heavy metal-free zeolite with low aluminum dissolution under gastric acid conditions, strong adsorption performance of harmful heavy metals, and excellent hemostatic performance.
[0012] (II) Technical solution
[0013] To achieve the above object, the present invention provides the following technical solution: a method for manufacturing activated zeolite without harmful heavy metals, comprising the following specific operating steps:
[0014] S1: Select alkali-modified and unblocked natural zeolite and prepare a solution with the natural zeolite. The solid content of the prepared solution is 1%-50%. Use alkali to adjust the pH of the solution system to maintain between 12.5-13.5 and stir.
[0015] S2: Phosphoric acid is added while the solution is stirred to maintain the pH value of the solution between 5.0 and 8.5 for reaction. After the reaction, the solution is repeatedly washed until the pH value of the washing solution is neutral, and then the modified natural zeolite is separated from the solution.
[0016] S3: Take the modified natural zeolite obtained above and prepare a solution, the solid content of the modified natural zeolite in the solution is 1%-50%, take ferrous salt and dissolve it in hydrochloric acid to prepare a solution, then add hydroxylamine hydrochloride, mix the modified natural zeolite solution with the ferrous salt, hydrochloric acid and hydroxylamine hydrochloride solution, and adjust the pH value of the solution to between 2.5 and 4 with acetic acid to react for a period of time.
[0017] S4: adding a complexing agent to the mixed solution after step S3, adjusting the pH value of the solution to between 1.0 and 4.0 with acetic acid, stirring and reacting for a period of time, separating the modified natural zeolite from the solution, and then repeatedly washing until the pH value of the washing solution is neutral and separating again.
[0018] S5: After the modified natural zeolite is separated from the solution, the obtained solution is mixed with the above solution to which the oxidant is added, and stirred for reaction, and an alkali solution is added to separate the harmful heavy metal precipitate from the solution.
[0019] S6: The modified natural zeolite free of heavy metals is prepared into a solution with a solid content of 1-50%, and calcium ions, iron ions and zinc ions are added to modify the natural zeolite free of heavy metals. Finally, the modified natural zeolite is separated from the solution, and then repeatedly washed until the pH value of the washing solution is neutral and separated again; the obtained modified natural zeolite free of harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite free of harmful heavy metals.
[0020] As a further embodiment of the present invention, the alkali used in step S1 is sodium hydroxide, potassium hydroxide or ammonia water.
[0021] As a further embodiment of the present invention, the separation method in steps S3 and S4 is to allow the mixture to settle naturally for 6-24 hours and then filter and separate, or to filter and separate by centrifugation.
[0022] As a further embodiment of the present invention, the oxidant in step S5 is set to one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0023] As a further feature of the present invention, the molar mass ratio of ferrous ions to hydroxylamine hydrochloride in step S3 is 10:1-100:1, and the mass ratio of modified natural zeolite to ferrous ions in the modified natural zeolite solution and the mixed solution of ferrous salt and hydroxylamine hydrochloride is 5:1-100:1.
[0024] As a further feature of the present invention, the complexing agent in S4 is set to be one or more complexing agents or chelating agents, and the mass ratio of the modified natural zeolite to the complexing agent or chelating agent is 10:1-200:1.
[0025] As a further embodiment of the present invention, the chelating agent includes but is not limited to citric acid, ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetic acid, diethylenetriamine pentatriacetic acid and diethyltriacetic acid, organic acid and phytic acid, and the complexing agent includes but is not limited to nitrilotriacetic acid and hydroxyethylenediaminetriacetic acid.
[0026] (III) Beneficial effects
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The present invention firstly uses an alkaline solution to modify the natural zeolite. The alkaline solution not only effectively dredges the natural zeolite pores and increases the specific surface area of the natural zeolite, but also significantly reduces the aluminum dissolution of the natural zeolite in the gastric acid solution system, and promotes the dissolution of harmful heavy metal arsenic in the natural zeolite; phosphoric acid is used to adjust the pH value of the solution reaction system, and the increase in the concentration of phosphate ions in the solution significantly realizes that the phosphate ions replace the arsenate ions of the same family in the natural zeolite into the solution, and further removes the harmful heavy metal arsenic in the natural zeolite. The harmful heavy metal arsenic is dissolved from the natural zeolite into the solution system to facilitate the separation of the natural zeolite from the solution. The modified natural zeolite can be separated from the solution by simply standing and naturally precipitating to remove the supernatant and filtering, or centrifuging; the obtained modified natural zeolite is added with an appropriate amount of ionized water and stirred, and then stood and naturally precipitated to remove the supernatant and then filtered, or centrifuged to achieve the cleaning of the natural zeolite. The production equipment is simple and very easy to operate. The modified natural zeolite can greatly reduce the phosphate content by cleaning.
[0029] The invention allows other harmful heavy metals in the natural zeolite to be continuously dissolved out, and then the modified natural zeolite and the harmful heavy metals can be completely separated by standing for natural precipitation, discarding the supernatant, filtering or centrifuging. The solution and washing liquid separated from the modified natural zeolite are mixed with the above-mentioned solution added with an oxidant to achieve oxidation of highly toxic trivalent arsenic into low toxic pentavalent arsenic, and oxidation of ferrous ions into ferric ions. The low solubility of ferric arsenate is fully utilized to achieve precipitation and recovery of some harmful heavy metals, thereby avoiding environmental pollution.
[0030] Ferrous zeolite is prepared by modifying natural zeolite with ferrous ions. Under the joint action of hydroxylamine hydrochloride and ferrous ions, the insoluble harmful heavy metal arsenic in natural zeolite is further reduced and dissolved to form relatively highly soluble arsenite, which significantly realizes the dissolution of various bound arsenic and insoluble arsenic in natural zeolite and their stable existence in the solution system, and realizes the physical separation of natural zeolite and harmful heavy metal arsenic; adding an appropriate amount of complexing agent or chelating agent under acidic conditions significantly realizes the dissolution and separation of other heavy metals from natural zeolite. After the natural zeolite is modified with calcium ions, iron ions and zinc ions and separated from the solution, it is repeatedly washed and dried and then calcined at high temperature to further dredge the pores of the natural zeolite. The multi-step reaction process is carried out at room temperature or with appropriate heating, and the reaction process is mild. The supernatant is removed by standing and natural sedimentation and then filtered or centrifuged. The production process is simple and easy to operate, with low equipment investment and low energy consumption.
[0031] The natural zeolite is modified by alkaline solution and the pores are unblocked, the natural zeolite is modified by hydroxylamine hydrochloride and ferrous ions, the natural zeolite is treated with chelating agents and complexing agents, and finally the natural zeolite is modified by calcium, iron and zinc ions. It is dried and activated at high temperature. The obtained modified natural zeolite without harmful heavy metals has significantly reduced aluminum dissolution under simulated gastric acid solution conditions, and basically does not adsorb iron ions, calcium ions and zinc ions added in the simulated gastric acid solution, and the hemostatic effectiveness is maintained well, the specific surface area is significantly increased, and the harmful heavy metals lead, arsenic, mercury and cadmium in the natural zeolite are significantly reduced or completely eliminated. As a raw material for feed and cosmetics, it can significantly reduce the content of harmful heavy metals in feed and cosmetics, improve product quality, and has significant social value. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0033] Implementation method 1:
[0034] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 11.5-13.5, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0035] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+ The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, and the mass ratio of modified natural zeolite to ferrous ion in the mixed solution is 5:1-100:1. The pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or under heating for 8-24 hours. Then, an appropriate amount of EDTA is added to the mixed solution. The mass ratio of modified natural zeolite to EDTA is 10:1-200:1, the pH value of the solution is adjusted to between 1.0-4.0 with hydrochloric acid or acetic acid, the ionic strength of the solution is adjusted with sodium chloride, the reaction is stirred at room temperature or heated appropriately for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing liquid is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed and stirred with the above-mentioned solution with the addition of the oxidant, and an appropriate amount of alkali solution is added to facilitate the precipitation of harmful heavy metals in the solution and separation from the solution to avoid harmful heavy metals from polluting the environment.
[0036] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0037] Implementation Method 2:
[0038] The invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 8.5-11.0, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0039] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, and the mass ratio of modified natural zeolite to ferrous ion in the mixed solution is 5:1-100:1. The pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or under heating for 8-24 hours. Then, an appropriate amount of EDTA is added to the mixed solution. The mass ratio of modified natural zeolite to EDTA is 10:1-200:1, the pH value of the solution is adjusted to between 1.0-4.0 with hydrochloric acid or acetic acid, the ionic strength of the solution is adjusted with sodium chloride, the reaction is stirred at room temperature or heated appropriately for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing liquid is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed and stirred with the above-mentioned solution with the addition of the oxidant, and an appropriate amount of alkali solution is added to facilitate the precipitation of harmful heavy metals in the solution and separation from the solution to avoid harmful heavy metals from polluting the environment.
[0040] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0041] The difference between implementation method 2 and implementation method 1 is that the amount of alkali solution modified natural zeolite added is insufficient. After the amount of alkali solution added is reduced, the pH value range of the solution decreases, and the pH value range is reduced from 11.5-13.0 in implementation method 1 to 8.5-11.0 in implementation method 2. Other experimental conditions are the same. The aluminum content of the obtained modified natural zeolite without (low) harmful heavy metals is increased from 0.01 mg / g in implementation method 1 to 2.30 mg / g in implementation method 2 under gastric acid solution conditions.
[0042] Implementation method 3:
[0043] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 11.5-13.5, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 9.0-11.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0044] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+ The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, and the mass ratio of modified natural zeolite to ferrous ion in the mixed solution is 5:1-100:1. The pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or under heating for 8-24 hours. Then, an appropriate amount of EDTA is added to the mixed solution. The mass ratio of modified natural zeolite to EDTA is 10:1-200:1, the pH value of the solution is adjusted to between 1.0-4.0 with hydrochloric acid or acetic acid, the ionic strength of the solution is adjusted with sodium chloride, the reaction is stirred at room temperature or heated appropriately for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing liquid is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed and stirred with the above-mentioned solution with the addition of the oxidant, and an appropriate amount of alkali solution is added to facilitate the precipitation of harmful heavy metals in the solution and separation from the solution to avoid harmful heavy metals from polluting the environment.
[0045] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0046] The difference between implementation method 3 and implementation method 1 is that after the alkali-modified natural zeolite reacts for a certain period of time, the amount of phosphoric acid added decreases and the pH value of the solution rises; that is, after the alkali-modified natural zeolite reacts for a period of time, less phosphoric acid is added, and the pH value range of the solution with insufficient addition of phosphoric acid is adjusted from the pH value of 5.0-8.5 in implementation method 1 to 9.0-11.5 in implementation method 3. The harmful heavy metal arsenic content of 3.39 mg / g in the natural zeolite obtained in implementation method 3 is higher than the harmful heavy metal arsenic content of 0.48 mg / g in implementation method 1. The main reason is that the concentration of phosphate ions is not high, resulting in insufficient replacement of harmful heavy metal arsenic of the same family.
[0047] Implementation Method 4:
[0048] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 11.5-13.5, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0049] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+The concentration of 0.1-2M) is dissolved in hydrochloric acid to prepare a solution, the natural zeolite solution is mixed with the ferrous solution, the mass ratio of the modified natural zeolite to the ferrous ion in the mixed solution is 5:1-100:1, the pH value of the solution is adjusted to between 2.5 and 4 with saline or acetic acid, and the reaction is carried out at room temperature or by heating for 8-24 hours; then an appropriate amount of EDTA is added to the mixed solution, the mass ratio of the modified natural zeolite to EDTA is 10:1-200:1, the pH value of the solution is adjusted to between 1.0 and 4.0 with hydrochloric acid or acetic acid, the ionic strength of the solution is adjusted with sodium chloride, the room temperature is stirred or the reaction is appropriately heated for 8-24 hours, and the natural zeolite is separated from the solution, for example, the natural precipitation is allowed to stand for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing solution is neutral, and then the natural precipitation is filtered to remove the supernatant and then filtered, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed with the above solution with the oxidant added, stirred and reacted, and an appropriate amount of alkali solution is added to precipitate harmful heavy metals in the solution to facilitate separation from the solution, thereby avoiding harmful heavy metals from polluting the environment.
[0050] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0051] The difference between implementation method 4 and implementation method 1 is that the weak oxidant hydroxylamine hydrochloride is not added to the ferrous salt solution, and the other reaction conditions are the same. In implementation method 4, the chelating agent EDTA solution is added to react for a period of time, and the solution is taken for detection and it is found that the solution contains a certain amount of trivalent iron; the modified natural zeolite without (low) harmful heavy metals is finally obtained. The harmful heavy metal arsenic content of the natural zeolite obtained by implementation method 4 is 6.44 mg / g, which is higher than 0.48 mg / g in implementation method 1. The harmful heavy metal removal of implementation method 4 is not as good as that of implementation method 1. The main reason may be that the dissolved harmful heavy metal arsenic re-forms new precipitation with iron ions and mixes in the natural zeolite.
[0052] Implementation method 5:
[0053] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 11.5-13.5, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0054] The obtained modified natural zeolite is then prepared into a solution with a solid content of 1%-10%, and then an appropriate amount of hydroxylamine hydrochloride (NH2OH.HCl) is added, and the mass ratio of the modified natural zeolite solution to the hydroxylamine hydrochloride is 10:1-200:1; the pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or by heating for 8-24 hours; then an appropriate amount of EDTA is added to the mixed solution, and the mass ratio of the modified natural zeolite to EDTA is 10:1-200:1, the pH value of the solution is adjusted to 1.0-4.0 with hydrochloric acid or acetic acid, and the ionic strength of the solution is adjusted with sodium chloride, and the reaction is carried out at room temperature or by appropriate heating for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours, the supernatant is removed and then filtered, or the supernatant is removed after centrifugation, and then water is added for repeated washing until the pH value of the washing solution is neutral, and then the solution is naturally precipitated and filtered to remove the supernatant, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed with the above solution with the oxidant added, stirred and reacted, and an appropriate amount of alkali solution is added to precipitate harmful heavy metals in the solution to facilitate separation from the solution, thereby avoiding harmful heavy metals from polluting the environment.
[0055] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0056] The difference between implementation method 5 and implementation method 1 is that no ferrous ion is added to modify the natural zeolite, only hydroxylamine hydrochloride is added, and the other reaction conditions are the same. The final modified natural zeolite without (low) harmful heavy metals has a harmful heavy metal arsenic content higher than 0.48 mg / g in implementation method 1, which is 7.73 mg / g in implementation method 5. The harmful heavy metal removal of implementation method 5 is not as good as that of implementation method 1. The main reason is that there is no ferrous ion-modified natural zeolite in the natural zeolite solution, and the single hydroxylamine hydrochloride cannot dissolve the insoluble harmful heavy metal arsenic in the natural zeolite, so the harmful heavy metal arsenic content in the natural zeolite is still high.
[0057] Implementation Method 6:
[0058] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the sodium hydroxide solubility is 1M-2M, the solid content of natural zeolite solution is 1%-10%, and the pH value of the solution system is adjusted by sodium hydroxide solution and maintained between 11.5-13.5, and stirred and reacted for 8-24 hours at room temperature or appropriately heated. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, and the solution is stirred or appropriately heated for 8-24 hours.
[0059] Take an appropriate amount of ferrous salt (Fe 2+ The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, and the mass ratio of modified natural zeolite to ferrous ion in the mixed solution is 5:1-100:1. The pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or under heating for 8-24 hours. Then, an appropriate amount of EDTA is added to the mixed solution. The mass ratio of modified natural zeolite to EDTA is 10:1-200:1, the pH value of the solution is adjusted to between 1.0-4.0 with hydrochloric acid or acetic acid, the ionic strength of the solution is adjusted with sodium chloride, the reaction is stirred at room temperature or heated appropriately for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing liquid is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed and stirred with the above-mentioned solution with the addition of the oxidant, and an appropriate amount of alkali solution is added to facilitate the precipitation of harmful heavy metals in the solution and separation from the solution to avoid harmful heavy metals from polluting the environment.
[0060] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0061] The difference between implementation method 6 and implementation method 1 is that the alkali-modified natural zeolite is reacted for a period of time, phosphoric acid is added and reacted for another period of time, and the phosphate-containing solution is not separated from the natural zeolite, and hydroxylamine hydrochloride and ferrous salt are directly added to continue the reaction; a large amount of phosphate ions in the solution of implementation method 6 are very easy to react with ferrous ions to form precipitation, which greatly affects the ferrous ion modification of natural zeolite and affects the dissolution and dissolution of the insoluble harmful heavy metal arsenic in natural zeolite. Therefore, the modified (low) harmful heavy metal arsenic content of 6.15 mg / g obtained by implementation method 6 is higher than the harmful heavy metal arsenic content of 0.48 mg / g in implementation method 1.
[0062] Implementation method 7:
[0063] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 11.5-13.5, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0064] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, and the mass ratio of modified natural zeolite to ferrous ion in the mixed solution is 5:1-100:1. The pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or under heating for 8-24 hours. Then, an appropriate amount of EDTA is added to the mixed solution. The mass ratio of modified natural zeolite to EDTA is 10:1-200:1, the pH value of the solution is adjusted to between 1.0-4.0 with hydrochloric acid or acetic acid, the ionic strength of the solution is adjusted with sodium chloride, the reaction is stirred at room temperature or heated appropriately for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing liquid is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed and stirred with the above-mentioned solution with the addition of the oxidant, and an appropriate amount of alkali solution is added to facilitate the precipitation of harmful heavy metals in the solution and separation from the solution to avoid harmful heavy metals from polluting the environment.
[0065] The modified natural zeolite is separated from the solution, for example, by standing and naturally settling for 6-24 hours to remove the supernatant and then filtering, or centrifuging to remove the supernatant, then adding water to wash repeatedly until the pH value of the washing solution is neutral, then naturally settling to remove the supernatant and then filtering or centrifuging to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0066] The difference between Implementation Method 7 and Implementation Method 1 is that the natural zeolite for removing harmful heavy metals has not been modified with iron ions, calcium ions and zinc ions. Compared with Implementation Method 1, the modified natural zeolite without (low) harmful heavy metals obtained by Implementation Method 7 has a similar removal of harmful heavy metals such as lead, arsenic, mercury, and cadmium as Implementation Method 1. However, in simulated gastric acid solution, the modified natural zeolite without (low) harmful heavy metals obtained by Implementation Method 7 has a certain adsorption of calcium, zinc, and iron ions, and oral administration into the human body may reduce the concentration of calcium, iron, and zinc ions that are beneficial to the human body.
[0067] Implementation Method 8:
[0068] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solid content of natural zeolite solution is 1%-10%, and a proper amount of ammonia gas or a proper amount of ammonia water is added into the solution to adjust the pH value of the solution system and maintain it between 11.5-13.5, and stir and react for 8-24 hours at room temperature or by appropriate heating. The solution is stirred and a proper amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, and the reaction is carried out at room temperature or by appropriate heating for 8-24 hours; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24 hours to remove the supernatant and then filtering, or centrifugation to remove the supernatant, and then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, and after the natural zeolite is separated from the solution, the solution and washing liquid are collected and a proper amount of oxidant is added and stirred appropriately for use, and the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0069] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+ The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, and the mass ratio of modified natural zeolite to ferrous ion in the mixed solution is 5:1-100:1. The pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or under heating for 8-24 hours. Then, an appropriate amount of EDTA is added to the mixed solution. The mass ratio of modified natural zeolite to EDTA is 10:1-200:1, the pH value of the solution is adjusted to between 1.0-4.0 with hydrochloric acid or acetic acid, the ionic strength of the solution is adjusted with sodium chloride, the reaction is stirred at room temperature or heated appropriately for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing liquid is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed and stirred with the above-mentioned solution with the addition of the oxidant, and an appropriate amount of alkali solution is added to facilitate the precipitation of harmful heavy metals in the solution and separation from the solution to avoid harmful heavy metals from polluting the environment.
[0070] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0071] The difference between Implementation Method 8 and Implementation Method 1 is that the alkali solution used to modify the natural zeolite is ammonia gas or ammonia water. Other conditions are the same. The harmful heavy metals and performance of the modified natural zeolite without (low) harmful heavy metals obtained by Implementation Method 8 are not significantly different from those of Implementation Method 1, indicating that the key to the alkali solution modified zeolite to remove harmful heavy metal arsenic and reduce aluminum dissolution lies in the pH value range of the solution.
[0072] Implementation Method 9:
[0073] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 11.5-13.5, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0074] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, wherein the mass ratio of the modified natural zeolite to the ferrous ion is 5:1-100:1, and the pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or under heating for 8-24 hours; an appropriate amount of disodium EDTA and citric acid are added to the mixed solution, and the ... under room temperature or under heating for 8-24 hours. The mass ratio of natural zeolite to disodium EDTA and citric acid is 10:1:1-200:1:1. The pH value of the solution is adjusted to between 1.0 and 4.0 with hydrochloric acid or acetic acid, and the ionic strength of the solution is adjusted with sodium chloride. The solution is stirred at room temperature or heated appropriately for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing liquid is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed and stirred with the above-mentioned solution with the addition of the oxidant, and an appropriate amount of alkali solution is added to facilitate the precipitation of harmful heavy metals in the solution and separation from the solution to avoid harmful heavy metals from polluting the environment.
[0075] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0076] The difference between Implementation Method 9 and Implementation Method 1 is that different complexing agents or chelating agents are used. Other conditions are the same. The harmful heavy metals and performance of the modified natural zeolite without (low) harmful heavy metals obtained by Implementation Method 9 are not significantly different from those of Implementation Method 1, indicating that the combined use of one or several complexing agents or chelating agents can effectively remove other heavy metals in natural zeolite.
[0077] Implementation Method 10:
[0078] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 11.5-13.5, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0079] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+ The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, wherein the mass ratio of the modified natural zeolite to the ferrous ion is 5:1-100:1, and the pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or under heating for 8-24 hours; an appropriate amount of nitrilotriacetic acid (NTA) and hydroxyethylenediaminetriacetic acid (HEDTA) are added to the mixed solution, and the .... The mass ratio of natural zeolite to nitrilotriacetic acid (NTA) and hydroxyethylenediaminetriacetic acid (HEDTA) is 10:1:1-200:1:1, the pH value of the solution is adjusted to between 1.0 and 4.0 with hydrochloric acid or acetic acid, the ionic strength of the solution is adjusted with sodium chloride, the reaction is stirred at room temperature or heated appropriately for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing liquid is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed and stirred with the above-mentioned solution with the addition of an oxidant, and an appropriate amount of alkali solution is added to facilitate the precipitation of harmful heavy metals in the solution and separation from the solution, so as to avoid harmful heavy metals from polluting the environment.
[0080] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0081] The difference between implementation method 10 and implementation method 1 is that the complexing agent or chelating agent is different. Other conditions are the same. The harmful heavy metals and performance of the modified natural zeolite without (low) harmful heavy metals obtained by implementation method 9 are not significantly different from those of implementation method 1, indicating that different complexing agents or chelating agents used in combination can effectively remove other heavy metals in natural zeolite.
[0082] Implementation Method 11:
[0083] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 11.5-13.5, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0084] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, wherein the mass ratio of the modified natural zeolite to the ferrous ion is 5:1-100:1, and the pH value of the solution is adjusted to 2.5-4 with saline or acetic acid, and the reaction is carried out at room temperature or under heating for 8-24 hours; an appropriate amount of disodium EDTA and citric acid are added to the mixed solution, and the ... under room temperature or under heating for 8-24 hours. The mass ratio of zeolite to disodium EDTA and citric acid is 10:1:1-200:1:1. The pH value of the solution is adjusted to between 4.5 and 7.0 with hydrochloric acid, acetic acid or alkali solution. The ionic strength of the solution is adjusted with sodium chloride. The solution is stirred at room temperature or heated appropriately for 8-24 hours. The natural zeolite is then separated from the solution, for example, the solution is allowed to stand for natural precipitation for 6-24 hours to remove the supernatant and then filter, or the supernatant is removed after centrifugation, and then water is added to wash repeatedly until the pH value of the washing solution is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed and stirred with the above-mentioned solution with the addition of an oxidant, and an appropriate amount of alkali solution is added to facilitate the precipitation of harmful heavy metals in the solution and separation from the solution, so as to avoid harmful heavy metals from polluting the environment.
[0085] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0086] The only difference between implementation method 11 and implementation method 9 is that after the complexing agent or chelating agent is added, the pH value of the solution system in the reaction process is different, and the pH value range is adjusted from pH 1.0-4.0 in implementation method 9 to pH 4.5-7.0 in implementation method 11. The contents of other harmful heavy metals such as lead, mercury, and cadmium in the modified natural zeolite without (low) harmful heavy metals obtained by implementation method 11 are higher than those in implementation method 1, implementation method 9, and implementation method 10. This shows that the removal of other heavy metals in natural zeolite is greatly affected by the pH value of the solution.
[0087] Implementation Method 12:
[0088] The present invention firstly uses alkali (such as sodium hydroxide, potassium hydroxide, ammonia water) to modify natural zeolite, the solubility of sodium hydroxide is 1M-2M, the solid content of natural zeolite solution is 1%-10%, sodium hydroxide solution is used to adjust the pH value of the solution system and maintain it between 11.5-13.5, room temperature or appropriate heating, stirring reaction for 8-24h. The solution is stirred and an appropriate amount of phosphoric acid is added to maintain the pH value of the solution between 5.0-8.5, room temperature or appropriate heating reaction for 8-24h; the modified natural zeolite is separated from the solution, for example, standing for natural precipitation for 6-24h to remove the supernatant and then filtering, or centrifugation to remove the supernatant, then adding water to repeatedly wash until the pH value of the washing liquid is neutral, standing for natural precipitation, filtering or centrifugation, after the natural zeolite is separated from the solution, the solution and washing liquid are collected and an appropriate amount of oxidant is added and stirred appropriately for use, the oxidant is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
[0089] The obtained modified natural zeolite is added with water to form a solution with a solid content of 1%-10%. An appropriate amount of ferrous salt (Fe 2+ The modified natural zeolite solution is mixed with ferrous salt and hydroxylamine hydrochloride, wherein the mass ratio of the modified natural zeolite to the ferrous ion in the mixed solution is 5:1-100:1, and the pH value of the solution is adjusted to between 2.5 and 4 with saline or acetic acid, and the reaction is carried out at room temperature or by heating for 8-24 hours; the pH value of the solution is adjusted to between 1.0 and 4.0 with hydrochloric acid or acetic acid, and the ionic strength of the solution is adjusted with sodium chloride, and the reaction is carried out at room temperature or by heating for 8-24 hours, and then the natural zeolite is separated from the solution, for example, the natural precipitation is allowed to stand for 6-24 hours, the supernatant is removed and then filtered, or the supernatant is removed after centrifugation, and then water is added for repeated washing until the pH value of the washing solution is neutral, and then the supernatant is removed by natural precipitation and filtration, or the supernatant is removed after centrifugation. After the natural zeolite is separated from the solution, the obtained solution and washing liquid are mixed with the above solution with the oxidant added, stirred and reacted, and an appropriate amount of alkali solution is added to precipitate harmful heavy metals in the solution to facilitate separation from the solution, thereby avoiding harmful heavy metals from polluting the environment.
[0090] Take an appropriate amount of the above modified natural zeolite for heavy metal removal to prepare a solution with a solid content of 1-50%. Then add an appropriate amount of calcium ions, iron ions, and zinc ions to modify the natural zeolite for harmful heavy metal removal. Finally, separate the modified natural zeolite from the solution, for example, let it stand for natural precipitation for 6-24 hours to remove the supernatant and then filter it, or centrifuge to remove the supernatant, then add water to wash repeatedly until the pH value of the washing liquid is neutral, then naturally precipitate to remove the supernatant and then filter or centrifuge to remove the supernatant. The obtained modified natural zeolite without (low) harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite without (low) harmful heavy metals.
[0091] The significant difference between implementation method 12 and implementation method 9 is that no complexing agent or chelating agent is added, and other adjustments are the same. The content of harmful heavy metals lead, mercury, and cadmium in the modified natural zeolite without (low) harmful heavy metals obtained by implementation method 12 is significantly higher than that in implementation methods 1, 8, 9, and 10. It shows that complexing agents or chelating agents can significantly remove harmful heavy metals lead, mercury, and cadmium in natural zeolite.
[0092] For the rigor of the technology, the experimental test data are shown in the following table:
[0093] Table 1 Detection results of harmful heavy metals in natural zeolite raw materials (GB5009)
[0094]
[0095] Table 2 Detection results of harmful heavy metals in modified activated natural zeolite (GB5009)
[0096] No Lead content (mg / kg) Mercury content (mg / kg) Cadmium content (mg / kg) Total arsenic content (mg / kg) 1# 0.17 0.03 0.04 0.48 2# 0.13 0.02 0.04 0.53 3# 0.11 0.03 0.03 3.39 4# 0.09 0.03 0.02 6.44 5# 0.21 0.02 0.01 7.73 6# 3.13 1.01 1.12 6.15 7# 0.13 0.02 0.03 0.53 8# 0.15 0.02 0.02 0.42 9# 0.14 0.03 0.02 0.46 10# 0.11 0.02 0.01 0.41 11# 5.14 3.11 1.78 4.67 12# 15.18 5.22 3.01 0.49
[0097] Table 3 Zeolite raw material performance indicators
[0098]
[0099] Table 4 Performance indexes of modified activated zeolite
[0100]
[0101]
[0102] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for producing activated zeolite without harmful heavy metals, characterized in that: The specific steps are as follows: S1: Select alkali-modified and unblocked natural zeolite and prepare a solution with the natural zeolite. The solid content of the prepared solution is 1%-50%. Use alkali to adjust the pH of the solution system to maintain between 12.5-13.5 and stir. S2: Phosphoric acid is added while the solution is stirred to maintain the pH value of the solution between 5.0 and 8.5 for reaction. After the reaction, the solution is repeatedly washed until the pH value of the washing solution is neutral, and then the modified natural zeolite is separated from the solution. S3: Take the modified natural zeolite obtained above and prepare a solution, the solid content of the modified natural zeolite in the solution is 1%-50%, take ferrous salt and dissolve it in hydrochloric acid to prepare a solution, then add hydroxylamine hydrochloride, mix the modified natural zeolite solution with the ferrous salt, hydrochloric acid and hydroxylamine hydrochloride solution, and adjust the pH value of the solution to between 2.5 and 4 with acetic acid to react for a period of time. S4: adding a complexing agent to the mixed solution after step S3, adjusting the pH value of the solution to between 1.0 and 4.0 with acetic acid, stirring and reacting for a period of time, separating the modified natural zeolite from the solution, and then repeatedly washing until the pH value of the washing solution is neutral and separating again. S5: After the modified natural zeolite is separated from the solution, the obtained solution is mixed with the above solution to which the oxidant is added, and stirred for reaction, and an alkali solution is added to separate the harmful heavy metal precipitate from the solution. S6: The modified natural zeolite free of heavy metals is prepared into a solution with a solid content of 1-50%, and calcium ions, iron ions and zinc ions are added to modify the natural zeolite free of heavy metals. Finally, the modified natural zeolite is separated from the solution, and then repeatedly washed until the pH value of the washing solution is neutral and separated again; the obtained modified natural zeolite free of harmful heavy metals is dried at 110°C, and then activated and modified at 350°C-550°C to obtain activated natural zeolite free of harmful heavy metals.
2. A method for producing activated zeolite without harmful heavy metals according to claim 1, characterized in that: The alkali used in step S1 is sodium hydroxide, potassium hydroxide or ammonia water.
3. A method for producing a harmful heavy metal-free activated zeolite according to claim 1, characterized in that: The separation method in steps S3 and S4 is to allow the mixture to settle naturally for 6-24 hours and then filter and separate, or to filter and separate by centrifugation.
4. A method for producing activated zeolite without harmful heavy metals according to claim 3, characterized in that: The oxidant in step S5 is one or more of hydrogen peroxide, sodium percarbonate, ozone, sodium hypochlorite or potassium nitrate.
5. A method for producing activated zeolite without harmful heavy metals according to claim 4, characterized in that: The molar mass ratio of ferrous ions to hydroxylamine hydrochloride in step S3 is 10:1-100:1, and the mass ratio of modified natural zeolite to ferrous ions in the modified natural zeolite solution and the mixed solution of ferrous salt and hydroxylamine hydrochloride is 5:1-100:
1.
6. A method for producing activated zeolite without harmful heavy metals according to claim 4, characterized in that: The complexing agent in S4 is set to be one or more complexing agents or chelating agents, and the mass ratio of the modified natural zeolite to the complexing agent or chelating agent is 10:1-200:
1.
7. A method for producing activated zeolite without harmful heavy metals according to claim 6, characterized in that: The chelating agent includes but is not limited to citric acid, ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetic acid, diethylenetriamine pentatriacetic acid and diethyltriacetic acid, organic acid and phytic acid, and the complexing agent includes but is not limited to nitrilotriacetic acid and hydroxyethylenediaminetriacetic acid.
Citation Information
Patent Citations
Treatment method for heavy-metal-containing wastewater
CN105668856A
Compound composed of zeolite powder and manganese oxide and preparation method and application thereof
CN113004092A
Preparation method of supported catalyst for treating degradation-resistant wastewater through catalytic ozonation
CN114713280A
Process for the Production of Zeolitic Molecular Sieves
FR1490184A