Method for reducing chloride ion content of industrial-grade magnesium hydroxide
Through the combination of brine-ammonia-lime combined method and hydrothermal reaction, ammonium sulfate is used to regulate the hydrothermal reaction of magnesium hydroxide, which successfully reduces the chloride ion content in industrial-grade magnesium hydroxide, and solves the problem of the chloride ion content not meeting the standard. Problem, low-cost, low-energy consumption of high-quality magnesium hydroxide preparation has been achieved.
Patent Information
- Application Number
- CN202411008716.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to reduce the chloride ion content in industrial grade magnesium hydroxide efficiently and at low cost, resulting in a great impact on equipment corrosion and flame retardant performance. Common methods have high alkali consumption, large water usage, and complex operations. etc.
Magnesium hydroxide fine powder was prepared by brine-ammonia-lime combined method, and through high-temperature pretreatment and hydrothermal reaction, using ammonium sulfate as crystal growth regulator, controlling the hydrothermal reaction conditions to reduce the chloride ion content, and finally passing filtration and drying A low-chlorine magnesium hydroxide product was obtained.
The chloride ion content is lower than the national standard, which reduces process costs and avoids high-energy consumption operations. The process is simple and the equipment requirements are low. The obtained products meet the application requirements of high-end magnesium materials.
Smart Images

Figure CN118908249A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical production, and in particular to a method for reducing the chloride ion content of industrial-grade magnesium hydroxide. Background Art
[0002] As an important inorganic chemical product, magnesium hydroxide has excellent physical and chemical properties such as safety, non-toxicity, weak alkali pollution-free, high temperature resistance, and corrosion resistance. As an antibacterial agent, wastewater and waste gas treatment agent, and a new generation of flame retardant, it is widely used in flame retardants, environmental protection, medicine and other fields. At present, the chlorine content of industrial-grade magnesium hydroxide products prepared by the salt lake magnesium chloride ammonia method is an average of 0.4%-0.6%. The reason for the high chlorine content is that the growth process of magnesium hydroxide is not controlled during the precipitation of MgCl2·6H2O ammonia alkali, and the chlorine is wrapped in the Mg(OH)2 particles, and the Mg(OH)2 continues to agglomerate and grow, resulting in an increase in the Cl content.
[0003] The addition of chloride ions will have a negative impact on the crystallization, growth, morphology, and particle size of magnesium hydroxide crystals, and thus affect the application performance of magnesium hydroxide. For example, under conditions of high temperature and high pressure, chloride ions may be highly corrosive to equipment, shortening the service life of the equipment; in flame retardant applications of polymers such as plastics and rubber, it may affect the flame retardant properties and aging properties of the material. Studies have shown that chloride ions in ammonia-processed magnesium hydroxide may accelerate the aging process of composite materials. The national standard "Industrial Magnesium Hydroxide" (GB / T 3607-2007) requires that the chloride ion content in high-quality magnesium hydroxide is not more than 0.1%.
[0004] At present, the common methods for reducing the chloride ion content of magnesium hydroxide mainly include washing method, recrystallization method, electrochemical method, ammonia solution circulating washing centrifugal method, etc. Among them, the recrystallization method is a method of using strong alkali to promote the recrystallization of magnesium hydroxide and reduce the chloride content of magnesium hydroxide, which has the problems of high alkali consumption and energy consumption, and difficulty in subsequent magnesium hydroxide filtration; the washing method is to use multi-stage countercurrent washing to reduce chlorine, which has the problems of large water usage and high subsequent water treatment costs; the ammonia solution circulating washing centrifugal method to reduce chlorine has the disadvantages of cumbersome process operation, complex control and difficulty in operation.
[0005] Therefore, how to remove chloride ions in magnesium hydroxide efficiently and at low cost has become a technical problem that needs to be solved urgently in the process of preparing low-chloride magnesium hydroxide. Summary of the invention
[0006] In view of the defects of the prior art, the present invention provides a method for reducing the chloride ion content of industrial-grade magnesium hydroxide, which has low cost, simple process, good dechlorination effect and can ensure that the chloride ion content in high-quality magnesium hydroxide is lower than the national standard.
[0007] To solve the above technical problems, the present invention adopts the following technical solution: a method for reducing the chloride ion content of industrial-grade magnesium hydroxide, characterized in that the method is carried out according to the following steps:
[0008] Step 1: obtaining industrial-grade magnesium hydroxide fine powder prepared by a brine-ammonia-lime combined process;
[0009] Step 2: pretreating the industrial grade magnesium hydroxide raw material at high temperature;
[0010] Step 3: adding the pretreated industrial-grade magnesium hydroxide fine powder into an aqueous solution containing a crystal growth regulator to carry out a hydrothermal reaction, wherein the regulator is ammonium sulfate;
[0011] Step 4: Filter and dry the magnesium hydroxide slurry obtained in step 3 to obtain a low-chlorine magnesium hydroxide product.
[0012] In step 2, the industrial-grade magnesium hydroxide raw material is placed in a muffle furnace for pretreatment, and the control conditions are: the pretreatment temperature is 300-800° C., and the pretreatment time is 0.5-8 hours.
[0013] In step 3, the pretreated industrial-grade magnesium hydroxide fine powder is added to a mixed solution of ammonium sulfate and water for hydrothermal reaction under the following control conditions: ammonium sulfate concentration is 0.1-0.5 mol / L, magnesium hydroxide solid content is 5-30% (mass), hydrothermal reaction time is 2-8h, and hydrothermal reaction temperature is 100-220°C.
[0014] The industrial grade magnesium hydroxide fine powder in step 1 is based on the salt lake magnesium resource bischofite, which is prepared by the brine-ammonia-lime combined method, wherein the chlorine content is 0.4-0.6% (mass content, particle size D 50 5-6μm, calcium oxide content ≤0.05%, chloride content 0.4%-0.6%).
[0015] Preferably, the pretreatment temperature in step 2 is 400-600° C., and the pretreatment time is 2-3 h.
[0016] Preferably, in step 3, the concentration of ammonium sulfate is 0.2-0.3 mol / L, the solid content of magnesium hydroxide is 10-20% (mass), the hydrothermal reaction time is 4-6h, and the hydrothermal reaction temperature is 120-180°C.
[0017] In step 4, the drying temperature is 60-80° C., and the chloride ion content of the obtained low-chlorine magnesium hydroxide product is as low as 0.0043 wt %.
[0018] The present invention adopts a combination of magnesium hydroxide pretreatment and crystal growth regulation to significantly reduce the chloride ion content in magnesium hydroxide. The chloride ion content can be as low as 0.0043wt%, which is far lower than the requirement of the chloride ion content in high-quality magnesium hydroxide of the national standard "Industrial Magnesium Hydroxide" (GB / T 3607-2007), and solves the pain points of the current industrial-grade magnesium hydroxide chloride content not meeting the standard and the limited application of downstream high-end magnesium materials.
[0019] At the same time, ammonium sulfate will dissociate into ammonium ions (NH4 + ), which increases the ionic strength of the solution and reacts with the hydroxyl groups (OH - ) reacts to accelerate the dissolution of magnesium oxide, while SO4 2- It can reduce the pH of the solution and further promote the hydration of magnesium oxide. 2+ With OH - Recrystallization forms magnesium hydroxide precipitation, and hydrothermal conditions are used to control the recrystallization of magnesium hydroxide, resulting in a low-chlorine and high-purity magnesium hydroxide product. This process has mild process conditions and low requirements for equipment and operation. It does not require high-energy-consuming operation units such as ball milling and multi-stage calcination in traditional dechlorination processes, and the process is green and energy-saving. In this way, the cost of the entire process can be reduced to 50-60% of the traditional process. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0021] The following is combined with Figure 1 The present invention is further described by specific embodiments:
[0022] Example 1
[0023] Weigh 10 g of industrial grade magnesium hydroxide (particle size D 50 5μm, calcium oxide content of 0.05%, chloride content of 0.4%). Magnesium hydroxide was spread in a crucible and placed in a muffle furnace for pretreatment, the pretreatment temperature was 300°C, and the pretreatment time was 0.5h. The pretreated industrial-grade magnesium hydroxide fine powder was then hydrothermally treated in a reactor, and magnesium hydroxide with a solid content of 10% was added to 0.2mol / L, 20mL of ammonium sulfate solution and 80mL of ultrapure water, the hydrothermal reaction temperature was 120°C, and the hydrothermal reaction time was 4h.
[0024] Results: The chloride ion content in the industrial grade magnesium hydroxide prepared was 0.016%.
[0025] Example 2
[0026] Weigh 10 g of industrial grade magnesium hydroxide (particle size D 505.5μm, calcium oxide content is 0, chloride content is 0.5%). Magnesium hydroxide is spread in a crucible and placed in a muffle furnace for pretreatment, the pretreatment temperature is 400°C, and the pretreatment time is 3h. The pretreated industrial-grade magnesium hydroxide fine powder is then hydrothermally treated in a reactor, and magnesium hydroxide with a solid content of 15% is added to 0.3mol / L, 40mL of ammonium sulfate solution and 60mL of ultrapure water, the hydrothermal reaction temperature is 160°C, and the hydrothermal reaction time is 5h.
[0027] Results: The chloride ion content in the industrial grade magnesium hydroxide prepared was 0.0043%.
[0028] Example 3
[0029] Weigh 10 g of industrial grade magnesium hydroxide (particle size D 50 5.2μm, calcium oxide content of 0.03%, chloride content of 0.5%). Magnesium hydroxide was spread in a crucible and placed in a muffle furnace for pretreatment at a temperature of 400°C for 2 hours. The pretreated industrial-grade magnesium hydroxide powder was then hydrothermally treated in a reactor, and magnesium hydroxide with a solid content of 12% was added to 0.2mol / L, 80mL of ammonium sulfate solution and 20mL of ultrapure water, with a hydrothermal reaction temperature of 150°C and a hydrothermal reaction time of 5 hours.
[0030] Results: The chloride ion content in the industrial grade magnesium hydroxide prepared was 0.015%.
[0031] Comparative Example
[0032] Weigh 10 g of industrial grade magnesium hydroxide (particle size D 50 6μm, calcium oxide content of 0.02%, chloride content of 0.6%). Magnesium hydroxide was spread in a crucible and placed in a muffle furnace for pretreatment, the pretreatment temperature was 400°C, and the pretreatment time was 2h. The pretreated industrial-grade magnesium hydroxide fine powder was then hydrothermally treated in a reactor, and magnesium hydroxide with a solid content of 10% was added to 100mL of ultrapure water, the hydrothermal reaction temperature was 160°C, and the hydrothermal reaction time was 4h.
[0033] Results: The chloride ion content in the industrial-grade magnesium hydroxide prepared was 0.24%, which was obviously higher than the chloride ion content in the industrial-grade magnesium hydroxide prepared by the method of the present invention.
[0034] The present invention has been described in detail above. The above description is only a preferred embodiment of the present invention and should not limit the scope of implementation of the present invention. That is, all equivalent changes and modifications made within the scope of this application should still fall within the scope of the present invention.
Claims
1. A method for reducing the chloride ion content of industrial grade magnesium hydroxide, characterized in that: Follow these steps: Step 1: obtaining industrial-grade magnesium hydroxide fine powder prepared by a brine-ammonia-lime combined process; Step 2: pretreating the industrial grade magnesium hydroxide raw material at high temperature; Step 3: adding the pretreated industrial-grade magnesium hydroxide fine powder into an aqueous solution containing a crystal growth regulator to carry out a hydrothermal reaction, wherein the regulator is ammonium sulfate; Step 4: Filter and dry the magnesium hydroxide slurry obtained in step 3 to obtain a low-chlorine magnesium hydroxide product.
2. The method for reducing the chloride ion content of industrial grade magnesium hydroxide according to claim 1, wherein: In step 2, the industrial-grade magnesium hydroxide raw material is placed in a muffle furnace for pretreatment, and the control conditions are: the pretreatment temperature is 300-800° C., and the pretreatment time is 0.5-8 h.
3. The method for reducing the chloride ion content of industrial grade magnesium hydroxide according to claim 1, wherein: In step 3, the pretreated industrial-grade magnesium hydroxide fine powder is added to a mixed solution of ammonium sulfate and water for hydrothermal reaction under the following control conditions: ammonium sulfate concentration is 0.1-0.5 mol / L, magnesium hydroxide solid content is 5-30%, hydrothermal reaction time is 2-8 h, and hydrothermal reaction temperature is 100-220° C.
4. The method for reducing the chloride ion content of industrial grade magnesium hydroxide according to claim 1, wherein: The industrial-grade magnesium hydroxide fine powder in step 1 is based on the salt lake magnesium resource bischofite, and is prepared by a brine-ammonia-lime combined process, wherein the chlorine content is 0.4-0.6%.
5. The method for reducing the chloride ion content of industrial grade magnesium hydroxide according to claim 2, wherein: The pretreatment temperature in step 2 is 400-600°C, and the pretreatment time is 2-3h.
6. The method for reducing the chloride ion content of industrial grade magnesium hydroxide according to claim 3, wherein: In step 3, the concentration of ammonium sulfate is 0.2-0.3 mol / L, the solid content of magnesium hydroxide is 10-20%, the hydrothermal reaction time is 4-6 hours, and the hydrothermal reaction temperature is 120-180°C.
7. The method for reducing the chloride ion content of industrial grade magnesium hydroxide according to claim 1, wherein: In step 4, the drying temperature is 60-80° C., and the chloride ion content of the obtained low-chlorine magnesium hydroxide product is as low as 0.0043 wt %.