Method for preparing hydrated magnesium carbonate crystal through magnesite hydrothermal one-step leaching
Through the one-step hydrothermal leaching method of magnesite, the process flow is simplified and energy consumption is reduced. The problems of uneven particle size and complex process of hydrated magnesium carbonate products in the existing technology are solved, and high-efficiency, high-quality and high-value hydrated magnesium carbonate crystal preparation is achieved. , suitable for high-end industrial applications.
Patent Information
- Application Number
- CN202410975417.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the development of magnesites has the phenomenon of enriched mining and abandoned poverty. The hydrated magnesium carbonate products produced are uneven in particle size, poor dispersion, irregular in shape, complex process and high energy consumption, making it difficult to meet the needs of high-end products.
The magnesium-rich ion solution is obtained by crushing, ball milling and hydrothermal leaching reactions, and then reacting with a carbon source to precipitate to form hydrated magnesium carbonate crystals with uniform particle size and dispersion, which simplifies the process flow , reduce energy consumption.
It has achieved efficient, high-quality and high-value utilization of magnesite resources. The hydrated magnesium carbonate crystals produced have uniform particle size, good dispersion and regular morphology. They are suitable for high-end industrial applications and significantly improve market competitiveness and economic benefits.
Smart Images

Figure CN118908251A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mineral processing technology and mineral material preparation, and particularly relates to a method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite. Background Art
[0002] my country has extremely rich magnesite resources, with proven reserves of about 3.58 billion tons. Over the years, my country's magnesite development has been seriously "mining the rich and abandoning the poor" and has been producing traditional magnesite refractory materials, magnesite building materials and other downstream products with low added value. The market competitiveness is weak, the low-end product capacity is in excess, and the high-end products rely on imports, which is far from meeting the urgent requirements of national economic development.
[0003] As an important new type of magnesium carbonate-based environmental mineral material, hydrated magnesium carbonate has the advantages of stable thermodynamic properties, non-toxicity, pollution-free, recyclability, and light weight. It is widely used as a polymer material, functional ceramics and glass, friction and carbon anode materials, food additives, biomedical carriers, templates for porous materials, etc. It has important industrial application value and has received much attention in the field of new materials.
[0004] However, the hydrated magnesium carbonate sold on the market is actually a low-end product obtained by simple physical crushing and calcination of natural minerals such as magnesite and dolomite. It has the disadvantages of large powder size, wide particle size distribution, serious agglomeration, irregular morphology, etc., which restricts its application range. In addition, domestic and foreign researchers currently mainly use high-purity chemical reagents such as magnesium chloride, magnesium sulfate, and magnesium nitrate as raw materials to prepare hydrated magnesium carbonate, which has high production costs and is difficult to industrialize. The preparation of hydrated magnesium carbonate using natural solid minerals as raw materials requires process flows such as crushing, grinding, high-temperature calcination, hydration, and carbonation, which has the disadvantages of complex process flow, high energy consumption, long cycle, and high cost.
[0005] Therefore, a method for leaching magnesium from magnesite with a simple process flow, low energy consumption and high efficiency, and the preparation of high-value-added hydrated magnesium carbonate crystals with uniform particle size distribution, good dispersibility and regular morphology will be of great significance for the efficient, high-value and high-quality comprehensive utilization of magnesite. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite. The method directly converts magnesite into a magnesium-rich solution, does not require high-temperature calcination, has low energy consumption, a simple process flow, and saves costs; in addition, the prepared hydrated magnesium carbonate crystals have the advantages of uniform particle size distribution, good dispersibility, regular morphology, etc., realizing efficient, high-quality, and high-value utilization of magnesite resources.
[0007] To achieve the above objectives, the technical solutions adopted in this application are as follows:
[0008] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0009] (1) Pretreatment
[0010] The magnesite ore is crushed, ball-milled, washed, and dried to obtain magnesite powder;
[0011] (2) Hydrothermal leaching reaction
[0012] Water is added to magnesite powder to prepare magnesite slurry, an organic acid is added to the slurry to obtain a mixed solution, a hydrothermal leaching reaction is performed, and a magnesium ion-rich solution is obtained after suction filtration;
[0013] (3) Precipitation reaction
[0014] A carbon source is introduced into a magnesium ion-rich solution, a precipitation reaction is carried out at 30-65° C., and a filter cake is washed and dried to obtain hydrated magnesium carbonate crystals.
[0015] in:
[0016] In the step (1), the magnesium oxide content in the magnesite is 45.0-47.0%, and the magnesite ore is ball-milled to 200-1000 meshes.
[0017] In the step (2), the mass ratio of water to magnesite in the magnesite slurry is (40-80):1.
[0018] In the step (2), the organic acid is selected from one of citric acid, oxalic acid, salicylic acid, p-hydroxybenzoic acid, m-hydroxybenzoic acid and sulfosalicylic acid, and the mass of the organic acid added is 1 to 8% of the mass of the slurry.
[0019] In the step (2), the organic acid is added in the form of powder or solution, and the mass of the organic acid in the solution is 1 to 8% of the mass of the slurry.
[0020] In the step (2), the hydrothermal leaching reaction temperature is 100 to 140° C., and the hydrothermal leaching reaction time is 0.5 to 3 hours.
[0021] In the step (2), the magnesium ion leaching rate in the magnesium ion-rich solution is ≥99.9%.
[0022] In the step (3), the carbon source is selected from one of sodium carbonate, sodium bicarbonate, ammonium carbonate and ammonium bicarbonate, and the molar ratio of magnesium ions in the magnesium ion-rich solution to carbonate ions in the carbon source is 1:(1-2).
[0023] In the step (3), the precipitation reaction time is 0.5 to 3 hours, and the stirring rate is 100 to 400 r / min.
[0024] In the step (3), the drying temperature is 50 to 70° C. and the drying time is 6 to 24 hours.
[0025] In the step (3), the particle size of the obtained hydrated magnesium carbonate crystals is 1 to 12 μm.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The present invention directly uses magnesite as raw material, which is rich in source and low in cost, and is an excellent raw material choice, and can replace chemical reagents such as magnesium sulfate, magnesium chloride, magnesium nitrate, and magnesium hydroxide.
[0028] 2. The present invention directly and efficiently leach magnesium from magnesite in one step, which can significantly reduce energy consumption, reduce environmental pollution, improve economic benefits, and has broad development prospects.
[0029] 3. The method for preparing hydrated magnesium carbonate crystals by hydrothermal leaching of magnesite of the present invention has a simple process flow and a short cycle, and hydrated magnesium carbonate crystals with uniform particle size distribution, regular morphology and good dispersibility can be obtained in a short time, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 A process flow chart of a method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite of the present invention;
[0031] Figure 2 XRD patterns of the hydrated magnesium carbonate prepared in Examples 1-3 of the present invention;
[0032] Figure 3 SEM image and particle size distribution diagram of hydrated magnesium carbonate prepared in Example 1 of the present invention;
[0033] Figure 4 SEM image and particle size distribution diagram of hydrated magnesium carbonate prepared in Example 2 of the present invention;
[0034] Figure 5 SEM image and particle size distribution diagram of the hydrated magnesium carbonate prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments.
[0036] The following provides a specific implementation method of the method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite of the present invention.
[0037] In the embodiment of the present invention, the organic acid and the carbon source are added in the form of powder.
[0038] Example 1
[0039] In this embodiment, the magnesium oxide content in the magnesite ore is 46.76%.
[0040] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, the process flow chart of which is as follows: Figure 1 As shown, the specific steps include:
[0041] (1) Pretreatment
[0042] The magnesite ore is crushed, ball-milled to 250 mesh, washed with water, and dried to obtain magnesite powder;
[0043] (2) Hydrothermal leaching reaction
[0044] The magnesite powder was moved into a reactor, and water was added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 70:1. 1.2% oxalic acid by mass of the slurry was added into the slurry, and then the reactor containing the mixed solution was moved into an oven for hydrothermal leaching reaction. The hydrothermal leaching reaction temperature was 140°C, and the hydrothermal leaching reaction time was 2h. After filtration, a magnesium ion-rich solution was obtained. The magnesium ion leaching rate was calculated to be 99.96% by EDTA titration method.
[0045] (3) Precipitation reaction
[0046] Ammonium carbonate was added to the magnesium-rich solution, the molar ratio of magnesium ions in the magnesium-rich solution to carbonate ions in ammonium carbonate was 1:1, and the precipitation reaction was carried out in a constant temperature water bath at 55°C for 1 hour with a stirring rate of 200 r / min. The filter cake was washed and dried at 50°C for 18 hours to obtain hydrated magnesium carbonate crystals.
[0047] The prepared hydrated magnesium carbonate crystals were analyzed, and their XRD patterns are shown in Figure 2 , SEM spectrum see Figure 3 .
[0048] from Figure 2 It can be seen that the diffraction peak of hydrated magnesium carbonate is consistent with the standard characteristic peak of magnesium carbonate trihydrate (JCPDS 70-1433), the diffraction peak intensity is high, the base is smooth, and no other impurity peaks appear, indicating that all the products are magnesium carbonate trihydrate.
[0049] from Figure 3 It can be seen that the product is rod-shaped magnesium carbonate trihydrate. The surface of the rod-shaped crystal is smooth, the length is 15 to 45 μm, the diameter is 1.5 to 5 μm, and the particle size distribution is mainly concentrated at 3.2±1.5 μm.
[0050] Example 2
[0051] In this embodiment, the magnesium oxide content in the magnesite ore is 46.76%.
[0052] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0053] (1) Pretreatment
[0054] The magnesite ore is crushed, ball-milled to 200 mesh, washed with water, and dried to obtain magnesite powder;
[0055] (2) Hydrothermal leaching reaction
[0056] The magnesite powder was moved into a reactor, and water was added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 50:1. 2.5% of salicylic acid by mass of the slurry was added into the slurry, and then the reactor containing the mixed solution was moved into an oven for hydrothermal leaching reaction. The hydrothermal leaching reaction temperature was 120°C, and the hydrothermal leaching reaction time was 1h. After filtration, a magnesium ion-rich solution was obtained. The magnesium ion leaching rate was calculated to be 99.98% by EDTA titration method.
[0057] (3) Precipitation reaction
[0058] Ammonium carbonate was added to the magnesium-rich solution, the molar ratio of magnesium ions in the magnesium-rich solution to carbonate ions in ammonium carbonate was 1:1, and the precipitation reaction was carried out in a constant temperature water bath at 65°C for 1.5 hours with a stirring rate of 150 r / min. The filter cake was washed and dried at 60°C for 12 hours to obtain hydrated magnesium carbonate crystals.
[0059] The prepared hydrated magnesium carbonate crystals were analyzed, and their XRD patterns are shown in Figure 2 , SEM spectrum see Figure 4 .
[0060] from Figure 2 It can be seen that the diffraction peak of hydrated magnesium carbonate is consistent with the standard characteristic peak of basic magnesium carbonate (JCPDS 70-0361), the diffraction peak intensity is high, the base is smooth, and no other impurity peaks appear, indicating that all the products are basic magnesium carbonate.
[0061] from Figure 3 It can be seen that the product is porous rod-shaped basic magnesium carbonate. The surface of the rod-shaped crystal is relatively rough, and it is assembled from plate-shaped crystals. Its length is 12 to 70 μm, its diameter is 5 to 15 μm, and its particle size distribution is mainly concentrated in 8.8±2.8 μm.
[0062] Example 3
[0063] In this embodiment, the magnesium oxide content in the magnesite ore is 45.89%.
[0064] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0065] (1) Pretreatment
[0066] The magnesite ore is crushed, ball-milled to 600 mesh, washed with water, and dried to obtain magnesite powder;
[0067] (2) Hydrothermal leaching reaction
[0068] The magnesite powder was moved into a reactor, and water was added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 50:1. 1.5% of the citric acid by mass of the slurry was added into the slurry, and then the reactor containing the mixed solution was moved into an oven for hydrothermal leaching reaction. The hydrothermal leaching reaction temperature was 100°C, and the hydrothermal leaching reaction time was 1.8h. After filtration, a magnesium ion-rich solution was obtained. The magnesium ion leaching rate was calculated to be 99.94% by EDTA titration method.
[0069] (3) Precipitation reaction
[0070] Ammonium carbonate was added to the magnesium-rich solution, the molar ratio of magnesium ions in the magnesium-rich solution to carbonate ions in ammonium carbonate was 1:1.5, and the precipitation reaction was carried out in a constant temperature water bath at 62°C for 1 hour with a stirring rate of 250 r / min. The filter cake was washed and dried at 60°C for 12 hours to obtain hydrated magnesium carbonate crystals.
[0071] The prepared hydrated magnesium carbonate crystals were analyzed, and their XRD patterns are shown in Figure 2 , SEM spectrum see Figure 5 .
[0072] from Figure 2 It can be seen that the diffraction peak of hydrated magnesium carbonate is consistent with the standard characteristic peak of basic magnesium carbonate (JCPDS 70-0361), the diffraction peak intensity is high, the base is smooth, and no other impurity peaks appear, indicating that all the products are basic magnesium carbonate.
[0073] from Figure 3 It can be seen that the product is a porous spherical basic magnesium carbonate, which is assembled from lamellar crystals with a diameter of about 8 μm and a particle size distribution mainly concentrated at 8.2±1.9 μm.
[0074] Example 4
[0075] In this embodiment, the magnesium oxide content in the magnesite ore is 45.89%.
[0076] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0077] (1) Pretreatment
[0078] The magnesite ore is crushed, ball-milled to 500 mesh, washed with water, and dried to obtain magnesite powder;
[0079] (2) Hydrothermal leaching reaction
[0080] The magnesite powder was moved into a reactor, and water was added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 65:1, and sulfosalicylic acid was added to the slurry at a mass ratio of 1% by mass of the slurry. Then, the reactor containing the mixed solution was moved into an oven for hydrothermal leaching reaction. The hydrothermal leaching reaction temperature was 100°C, and the hydrothermal leaching reaction time was 0.5h. After filtration, a magnesium ion-rich solution was obtained. The magnesium ion leaching rate was calculated to be 99.98% by EDTA titration method.
[0081] (3) Precipitation reaction
[0082] Ammonium carbonate was added to the magnesium-rich solution, the molar ratio of magnesium ions in the magnesium-rich solution to carbonate ions in ammonium carbonate was 1:1.5, and the precipitation reaction was carried out in a constant temperature water bath at 45°C for 3 hours with a stirring rate of 200 r / min. The filter cake was washed and dried at 70°C for 8 hours to obtain hydrated magnesium carbonate crystals.
[0083] Example 5
[0084] In this embodiment, the magnesium oxide content in the magnesite ore is 45.89%.
[0085] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0086] (1) Pretreatment
[0087] The magnesite ore is crushed, ball-milled to 500 mesh, washed with water, and dried to obtain magnesite powder;
[0088] (2) Hydrothermal leaching reaction
[0089] The magnesite powder was moved into a reactor, and water was added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 65:1, and 3% of the mass of p-hydroxybenzoic acid was added to the slurry, and then the reactor containing the mixed solution was moved into an oven for hydrothermal leaching reaction. The hydrothermal leaching reaction temperature was 140°C, and the hydrothermal leaching reaction time was 1h. After filtration, a magnesium ion-rich solution was obtained, and the magnesium ion leaching rate was calculated to be 99.95% by EDTA titration method;
[0090] (3) Precipitation reaction
[0091] Ammonium carbonate was added to the magnesium-rich solution, the molar ratio of magnesium ions in the magnesium-rich solution to carbonate ions in ammonium carbonate was 1:2, and the precipitation reaction was carried out in a constant temperature water bath at 45°C for 2 hours with a stirring rate of 200 r / min. The filter cake was washed and dried at 70°C for 10 hours to obtain hydrated magnesium carbonate crystals.
[0092] Example 6
[0093] In this embodiment, the magnesium oxide content in the magnesite ore is 45.89%.
[0094] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0095] (1) Pretreatment
[0096] The magnesite ore is crushed, ball-milled to 500 mesh, washed with water, and dried to obtain magnesite powder;
[0097] (2) Hydrothermal leaching reaction
[0098] The magnesite powder was moved into a reactor, and water was added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 65:1, and 6% of the mass of m-hydroxybenzoic acid was added to the slurry, and then the reactor containing the mixed solution was moved into an oven for hydrothermal leaching reaction. The hydrothermal leaching reaction temperature was 140°C, and the hydrothermal leaching reaction time was 1.5h. After filtration, a magnesium ion-rich solution was obtained. The magnesium ion leaching rate was calculated to be 99.97% by EDTA titration method.
[0099] (3) Precipitation reaction
[0100] Ammonium carbonate was added to the magnesium-rich solution, the molar ratio of magnesium ions in the magnesium-rich solution to carbonate ions in ammonium carbonate was 1:2, and the precipitation reaction was carried out in a constant temperature water bath at 65°C for 2 hours with a stirring rate of 200 r / min. The filter cake was washed and dried at 60°C for 12 hours to obtain hydrated magnesium carbonate crystals.
[0101] Comparative Example 1
[0102] In this embodiment, the magnesium oxide content in the magnesite ore is 46.76%.
[0103] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0104] (1) Pretreatment
[0105] The magnesite ore is crushed, ball-milled to 250 mesh, washed with water, and dried to obtain magnesite powder;
[0106] (2) Hydrothermal leaching reaction
[0107] The magnesite powder is transferred to a reactor, water is added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 70:1, 1.2% oxalic acid by mass of the slurry is added to the slurry, and then the reactor containing the mixed solution is transferred to room temperature for leaching for 48 hours, and a magnesium ion-containing solution is obtained after suction filtration;
[0108] (3) Precipitation reaction
[0109] Ammonium carbonate was added to the magnesium ion-containing solution, the molar ratio of magnesium ions in the magnesium ion-containing solution to carbonate ions in ammonium carbonate was 1:1, and the precipitation reaction was carried out in a constant temperature water bath at 55°C for 1 hour with a stirring rate of 200 r / min. The filter cake was washed and dried at 50°C for 18 hours to obtain hydrated magnesium carbonate crystals.
[0110] Comparative Example 2
[0111] In this embodiment, the magnesium oxide content in the magnesite ore is 46.76%.
[0112] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0113] (1) Pretreatment
[0114] The magnesite ore is crushed, ball-milled to 200 mesh, washed with water, and dried to obtain magnesite powder;
[0115] (2) Hydrothermal leaching reaction
[0116] The magnesite powder is transferred to a reactor, water is added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 50:1, 2.5% of salicylic acid by mass of the slurry is added to the slurry, and then the reactor containing the mixed solution is transferred to room temperature for leaching for 48 hours, and a magnesium ion-containing solution is obtained after suction filtration;
[0117] (3) Precipitation reaction
[0118] Ammonium carbonate was added to the magnesium ion-containing solution, the molar ratio of magnesium ions in the magnesium ion-containing solution to carbonate ions in ammonium carbonate was 1:1, and the precipitation reaction was carried out in a constant temperature water bath at 65°C for 1.5 hours with a stirring rate of 150 r / min. The filter cake was washed and dried at 60°C for 12 hours to obtain hydrated magnesium carbonate crystals.
[0119] Comparative Example 3
[0120] In this embodiment, the magnesium oxide content in the magnesite ore is 45.89%.
[0121] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0122] (1) Pretreatment
[0123] The magnesite ore is crushed, ball-milled to 600 mesh, washed with water, and dried to obtain magnesite powder;
[0124] (2) Hydrothermal leaching reaction
[0125] The magnesite powder is transferred to a reactor, water is added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 50:1, 1.5% of citric acid by mass of the slurry is added to the slurry, and then the reactor containing the mixed solution is transferred to room temperature for leaching for 48 hours, and a magnesium ion-containing solution is obtained after suction filtration;
[0126] (3) Precipitation reaction
[0127] Ammonium carbonate was added to the magnesium ion-containing solution, the molar ratio of magnesium ions in the magnesium ion-containing solution to carbonate ions in ammonium carbonate was 1:1.5, and the precipitation reaction was carried out in a constant temperature water bath at 62°C for 1 hour with a stirring rate of 250 r / min. The filter cake was washed and dried at 60°C for 12 hours to obtain hydrated magnesium carbonate crystals.
[0128] Comparative Example 4
[0129] In this embodiment, the magnesium oxide content in the magnesite ore is 45.89%.
[0130] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0131] (1) Pretreatment
[0132] The magnesite ore is crushed, ball-milled to 500 mesh, washed with water, and dried to obtain magnesite powder;
[0133] (2) Hydrothermal leaching reaction
[0134] The magnesite powder is transferred to a reactor, water is added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 65:1, sulfosalicylic acid is added to the slurry at a mass ratio of 1% by mass of the slurry, and then the reactor containing the mixed solution is transferred to room temperature for leaching for 48 hours, and a magnesium ion-containing solution is obtained after suction filtration;
[0135] (3) Precipitation reaction
[0136] Ammonium carbonate was added to the magnesium ion-containing solution, the molar ratio of magnesium ions in the magnesium ion-containing solution to carbonate ions in ammonium carbonate was 1:1.5, and the precipitation reaction was carried out in a constant temperature water bath at 45°C for 3 hours with a stirring rate of 200 r / min. The filter cake was washed and dried at 70°C for 8 hours to obtain hydrated magnesium carbonate crystals.
[0137] Comparative Example 5
[0138] In this embodiment, the magnesium oxide content in the magnesite ore is 45.89%.
[0139] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0140] (1) Pretreatment
[0141] The magnesite ore is crushed, ball-milled to 500 mesh, washed with water, and dried to obtain magnesite powder;
[0142] (2) Hydrothermal leaching reaction
[0143] The magnesite powder is transferred to a reactor, water is added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 65:1, 3% of the mass of p-hydroxybenzoic acid is added to the slurry, and then the reactor containing the mixed solution is transferred to room temperature for leaching for 48 hours, and a magnesium ion-containing solution is obtained after suction filtration;
[0144] (3) Precipitation reaction
[0145] Ammonium carbonate was added to the magnesium ion-containing solution, the molar ratio of magnesium ions in the magnesium ion-containing solution to carbonate ions in ammonium carbonate was 1:2, and the precipitation reaction was carried out in a constant temperature water bath at 45°C for 2 hours with a stirring rate of 200 r / min. The filter cake was washed and dried at 70°C for 10 hours to obtain hydrated magnesium carbonate crystals.
[0146] Comparative Example 6
[0147] In this embodiment, the magnesium oxide content in the magnesite ore is 45.89%.
[0148] A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, specifically comprising the following steps:
[0149] (1) Pretreatment
[0150] The magnesite ore is crushed, ball-milled to 500 mesh, washed with water, and dried to obtain magnesite powder;
[0151] (2) Hydrothermal leaching reaction
[0152] The magnesite powder is transferred to a reactor, water is added to prepare a magnesite slurry according to a mass ratio of water to magnesite of 65:1, 6% of the mass of m-hydroxybenzoic acid is added to the slurry, and then the reactor containing the mixed solution is transferred to room temperature for leaching for 48 hours, and a magnesium ion-containing solution is obtained after suction filtration;
[0153] (3) Precipitation reaction
[0154] Ammonium carbonate was added to the magnesium ion-containing solution, the molar ratio of magnesium ions in the magnesium ion-containing solution to carbonate ions in ammonium carbonate was 1:2, and the precipitation reaction was carried out in a constant temperature water bath at 65°C for 2 hours with a stirring rate of 200 r / min. The filter cake was washed and dried at 60°C for 12 hours to obtain hydrated magnesium carbonate crystals.
[0155] By adopting the process flow of comparative examples 1-6 and the EDTA titration method, the magnesium ion leaching rates were calculated to be 5.6%, 16.7%, 15.3%, 20.6%, 3.7% and 5.8%, respectively. There were disadvantages such as low leaching rate and long leaching time.
[0156] It can be seen from the above embodiments that in the process of preparing hydrated magnesium carbonate crystals, the present invention can efficiently leach the magnesium element in magnesite in one step of hydrothermal treatment, shorten the time, simplify the process flow, and reduce energy consumption, thereby achieving clean and efficient utilization of magnesite; the prepared hydrated magnesium carbonate particles have uniform size, good dispersibility, and regular morphology, and can be widely used in the field of inorganic chemical industry, significantly improving the added value of magnesite.
Claims
1. A method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite, characterized in that: The specific steps include: (1) Pretreatment The magnesite ore is crushed, ball-milled, washed, and dried to obtain magnesite powder; (2) Hydrothermal leaching reaction Water is added to magnesite powder to prepare magnesite slurry, an organic acid is added to the slurry to obtain a mixed solution, a hydrothermal leaching reaction is performed, and a magnesium ion-rich solution is obtained after suction filtration; (3) Precipitation reaction A carbon source is introduced into a magnesium ion-rich solution, a precipitation reaction is carried out at 30-65° C., and a filter cake is washed and dried to obtain hydrated magnesium carbonate crystals.
2. The method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite according to claim 1, characterized in that: In the step (1), the magnesium oxide content in the magnesite is 45.0-47.0%, and the magnesite ore is ball-milled to 200-1000 meshes.
3. The method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite according to claim 1, characterized in that: In the step (2), the mass ratio of water to magnesite in the magnesite slurry is (40-80):
1.
4. The method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite according to claim 1, characterized in that: In the step (2), the organic acid is selected from one of citric acid, oxalic acid, salicylic acid, p-hydroxybenzoic acid, m-hydroxybenzoic acid and sulfosalicylic acid, and the mass of the organic acid added is 1 to 8% of the mass of the slurry.
5. The method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite according to claim 1, characterized in that: In the step (2), the hydrothermal leaching reaction temperature is 100 to 140° C., and the hydrothermal leaching reaction time is 0.5 to 3 hours.
6. The method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite according to claim 1, characterized in that: In the step (2), the magnesium ion leaching rate in the magnesium ion-rich solution is ≥99.9%.
7. The method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite according to claim 1, characterized in that: In the step (3), the carbon source is selected from one of sodium carbonate, sodium bicarbonate, ammonium carbonate and ammonium bicarbonate, and the molar ratio of magnesium ions in the magnesium ion-rich solution to carbonate ions in the carbon source is 1:(1-2).
8. The method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite according to claim 1, characterized in that: In the step (3), the precipitation reaction time is 0.5 to 3 hours, and the stirring rate is 100 to 400 r / min.
9. The method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite according to claim 1, characterized in that: In the step (3), the drying temperature is 50 to 70° C. and the drying time is 6 to 24 hours.
10. The method for preparing hydrated magnesium carbonate crystals by hydrothermal one-step leaching of magnesite according to claim 1, characterized in that: In the step (3), the particle size of the obtained hydrated magnesium carbonate crystals is 1 to 12 μm.