Production method of rod-like boehmite

By regulating the Al3+ concentration and precipitant type, combined with the use of carboxylic acid modifier, the problem of difficult process conditions and product aggregation in boehmite preparation is solved, and the fine regulation and size uniformity of rod-shaped nanorods are achieved, which meets the Improved performance requirements.

CN118908257APending Publication Date: 2024-11-08ANHUI YISHITONG NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411005805.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing boehmite preparation methods, process conditions are difficult to control and products are prone to agglomeration, resulting in high production costs and insufficient controllability of size, making it difficult to meet the improvement of performance requirements.

Method used

By dissolving the aluminum-containing substance in a solution configured to a certain concentration in the solvent, adding a precipitant dropwise under stirring conditions, and adding a modifier to the hydrothermal reaction to regulate the Al3+ concentration and precipitant type, and using the curling growth mechanism to form a rod-shaped erection Molsil, a carboxylic acid modifier inhibits crystal growth and controls the size and morphology of nanorods.

Benefits of technology

The fine microstructure of boehmite is achieved. By adjusting the Al3+ concentration and precipitant type, it affects the crystal nucleus concentration and growth direction, inhibits crystal growth, and obtains rod-shaped nanorods with uniform size and good shape control, reducing production costs and process Complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004962981700000061
    Figure BDA0004962981700000061
  • Figure BDA0004962981700000071
    Figure BDA0004962981700000071
Patent Text Reader

Abstract

The invention discloses a rod-like boehmite production method, which specifically comprises: dissolving an aluminum-containing substance in a solvent to prepare a solution with a certain concentration, dropwise adding a precipitating agent under a stirring condition, transferring to a reaction kettle, carrying out a hydrothermal reaction, adding a modifying agent after the reaction is completed, and continuously carrying out the reaction to obtain the rod-like boehmite. After the reaction is finished, purifying to obtain the rod-like boehmite. The boehmite is prepared by adopting the method disclosed by the invention, the prepared microstructure can be finely regulated and controlled, and the method has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of inorganic material preparation, in particular to a method for producing rod-shaped boehmite. Background Art

[0002] As an important new material, boehmite is an important precursor material for the preparation of different crystalline forms of alumina. It has the characteristics of zero-point charge, high interfacial free energy, large porosity, large specific surface area, good dispersibility, good colloidal solubility and high heat resistance. It is widely used in adsorption separation, catalysis, composite materials, liquid crystal, medicine, optics, sensors and other fields.

[0003] The preparation methods of boehmite mainly include: direct aluminum hydrolysis method, aluminum alkoxide hydrolysis method, sol-gel method, water / solvothermal method and other methods.

[0004] The products of aluminum direct hydrolysis method have good crystallinity, short reaction time, simple process flow, low cost and environmental friendliness, but the process conditions are difficult to control, the aluminum powder is poor in safety and the products are seriously agglomerated. The aluminum alcohol salt hydrolysis process has purification, no pollution to the environment, and the alcohol can be recycled, but the boehmite obtained by this method in industrial production is prone to agglomeration, and it is necessary to use external mechanical force to open the nanoparticle agglomerates, which increases the process steps and production costs. The products of sol-gel method are uniformly dispersed, high in purity, small in particle size, etc., which are suitable for the preparation of nano-boehmite, but the reaction time is long, the production cost is high, and the agglomeration is serious during the post-treatment process. The water / solvothermal method has high purity, low agglomeration, simple process flow, easy operation, environmental friendliness and wide application, but with the increasing requirements for the performance of boehmite, the controllability of the structure and size of the prepared boehmite is also required. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for producing rod-shaped boehmite. The boehmite is prepared by the method of the present invention, and the prepared microstructure can be finely controlled.

[0006] The technical solution of the present invention is achieved in this way:

[0007] The present invention provides a method for producing rod-shaped boehmite, which specifically comprises the following steps:

[0008] The aluminum-containing substance is dissolved in a solvent to prepare a solution of a certain concentration, a precipitant is added dropwise under stirring, and then the solution is transferred to a reactor for hydrothermal reaction. After the reaction is completed, a modifier is added to continue the reaction, and after purification, the rod-shaped boehmite is obtained.

[0009] Furthermore, the aluminum-containing substance is an aluminum salt.

[0010] Furthermore, the aluminum-containing salt includes one or more of aluminum chloride and aluminum nitrate.

[0011] During the hydrothermal reaction, the formation process of boehmite is as follows: Al 3+ It reacts with alkaline precipitants to form amorphous Al(OH)3, which then dissolves and forms lamellar boehmite. In lamellar boehmite, each layer is connected by hydrogen bonds of hydroxyl groups. Under acidic conditions, protons in the solution will combine with O in the hydroxyl group through shared electron pairs to form water ligands, thus destroying the original lamellar structure. In order to reduce the energy of the system, the exfoliated nanosheets form rods through a curling growth mechanism.

[0012] Furthermore, the concentration is 0.02-0.16 mol·mL -1 .

[0013] Al 3+ When the concentration is low, the concentration of crystal nuclei formed in the reaction system is low. As the crystallization reaction proceeds, it is easy to crystallize larger particles on the existing grains, and nanorods with larger diameters are obtained through the curling growth mechanism. In addition, due to the decrease in the concentration of crystal nuclei, the probability of directional contact growth between nanorods is small, which increases the length difference. When the Al3+ concentration increases, the concentration of crystal nuclei formed in the reaction system increases, the diameter of the nanorods decreases, and the probability of directional contact growth increases. Therefore, the size of the resulting product is more uniform and the aspect ratio increases.

[0014] Furthermore, the precipitant is an alkaline substance.

[0015] Furthermore, the alkaline substance includes one or more of hydrazine hydrate, ammonia water, and sodium hydroxide.

[0016] The change of the type of alkaline precipitant mainly changes the OH - With Al 3+ The rate of the neutralization reaction of H+ produced by hydrolysis increases with the increase of the alkalinity of the precipitant, resulting in the formation of a large amount of Al(OH)3 in the reaction system, which increases the nucleation rate of boehmite nuclei, is beneficial to reducing the size of the grains in the reaction system, reducing the diameter of the initial boehmite nanorods, and directional contact growth between the grains, further increasing the aspect ratio of the nanorods.

[0017] Furthermore, the modifier is carboxylic acid.

[0018] Furthermore, the carboxylic acid is an alkyl carboxylic acid.

[0019] Boehmite has hydroxyl groups on the surface, and carboxylic acids can react / adsorb on the surface of boehmite, thereby inhibiting crystal growth on these surfaces. Therefore, crystals grow rapidly on surfaces without hydroxyl groups, changing the morphology of the product.

[0020] Furthermore, the hydrothermal reaction conditions are 120-200° C., 12 h.

[0021] The invention also provides a rod-shaped boehmite prepared by the method.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. Through Al 3+ Adjustment of concentration affects the concentration of crystal nuclei, thereby regulating the growth rate and direction of boehmite.

[0024] 2. Carboxylic acids can react / adsorb on the hydroxyl-containing surfaces of boehmite, thereby inhibiting the crystal growth on these surfaces and growing in the direction without hydroxyl groups, thereby obtaining boehmite of the desired shape.

[0025] The addition of alkyl carboxylic acids enhances the dissolution-recrystallization process of boehmite and inhibits the crystal growth along the minor axis of the particles. Due to the increase in the coverage of the surface modifier, the aspect ratio of the particles increases with the decrease in the length of the modifier alkyl chain. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described in combination with the embodiments below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Reagent Description:

[0028] Aluminum nitrate, hydrazine hydrate, ammonia, sodium hydroxide, alkyl carboxylic acid, analytical grade, Sinopharm Chemical Reagent Co., Ltd.

[0029] Example 1

[0030] Dissolve 2 mol aluminum nitrate in deionized water to a concentration of 0.02 mol·mL -1 The solution was stirred at 0.25 mL min -1 Hydrazine hydrate was added dropwise at a rate of 100 μg / mL until the solution pH value was 5, then transferred to a reactor and reacted at 200 °C for 12 h, and then 3 L of 1 mol·mL -1 The hexanoic acid was reacted for 4 hours, and after cooling to room temperature, it was washed by centrifugation with ethanol for 3 times, and dried at 70° C. for 3 hours to obtain the rod-shaped boehmite.

[0031] Example 2

[0032] The difference between this embodiment and embodiment 1 is that the concentration of aluminum nitrate is 0.04 mol.

[0033] The other parts are exactly the same as those in Example 1.

[0034] Example 3

[0035] The difference between this embodiment and embodiment 1 is that the concentration of aluminum nitrate is 0.06 mol.

[0036] The other parts are exactly the same as those in Example 1.

[0037] Example 4

[0038] The difference between this embodiment and embodiment 1 is that the concentration of aluminum nitrate is 0.08 mol.

[0039] The other parts are exactly the same as those in Example 1.

[0040] Example 5

[0041] The difference between this embodiment and embodiment 1 is that the concentration of aluminum nitrate is 0.16 mol.

[0042] The other parts are exactly the same as those in Example 1.

[0043] Example 6

[0044] The difference between this embodiment and embodiment 1 is that the precipitant is ammonia water.

[0045] The other parts are exactly the same as those in Example 1.

[0046] Example 7

[0047] The difference between this embodiment and embodiment 1 is that the precipitant is sodium hydroxide.

[0048] The other parts are exactly the same as those in Example 1.

[0049] Example 8

[0050] The difference between this embodiment and embodiment 1 is that the caproic acid concentration is 0.5 mol·mL -1 , the addition amount is 6L.

[0051] The other parts are exactly the same as those in Example 1.

[0052] Example 9

[0053] The difference between this embodiment and embodiment 1 is that the concentration of caproic acid is 1.5 mol·mL -1 , the addition amount is 2L.

[0054] The other parts are exactly the same as those in Example 1.

[0055] Example 10

[0056] The difference between this embodiment and embodiment 1 is that the alkyl carboxylic acid is octanoic acid.

[0057] The other parts are exactly the same as those in Example 1.

[0058] Embodiment 11

[0059] The difference between this embodiment and embodiment 1 is that the alkyl carboxylic acid is capric acid.

[0060] The other parts are exactly the same as those in Example 1.

[0061] Example 12

[0062] The difference between this embodiment and embodiment 1 is that the alkyl carboxylic acid is hexadecanoic acid. The other parts are exactly the same as those in embodiment 1.

[0063] Embodiment 13

[0064] The difference between this embodiment and embodiment 1 is that the alkyl carboxylic acid is octadecanoic acid. The other parts are exactly the same as those in embodiment 1.

[0065] Results and Testing

[0066] The diameter and length were measured and the aspect ratio was calculated. The results are shown in Table 1.

[0067] Table 1

[0068]

[0069]

[0070] It can be seen from Table 1 Examples 1-5 that with Al 3+ With the increase of concentration, the size distribution of nanorods becomes more uniform and the aspect ratio increases continuously.

[0071] It can be seen from Example 1 and Examples 6-7 in Table 1 that as the alkalinity of the added precipitant increases, the diameter of the obtained product decreases and the aspect ratio increases.

[0072] As can be seen from Table Example 1 and Examples 8-9, the enhancement of crystal growth becomes more obvious with increasing caproic acid concentration. A possible explanation for the accelerated crystal growth is that the reduction of boehmite increases the solubility of pH, which is caused by the addition of caproic acid. Under acidic conditions, the solubility of boehmite increases with decreasing pH. Since dissolution-recrystallization is promoted under high solubility conditions, faster crystal growth can be observed at lower pH values, i.e., at higher caprylic acid concentrations.

[0073] It can be seen from the table of examples and examples 10-13 that since the pKa of the modifier increases with the increase of the alkyl chain length, when a longer alkyl chain modifier is used, the pH of the reaction medium may be higher, which is not conducive to promoting the crystal growth of bohmite.

[0074] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for producing rod-shaped boehmite, characterized in that: The specific steps include: The aluminum-containing substance is dissolved in a solvent to prepare a solution of a certain concentration, a precipitant is added dropwise under stirring, and then the solution is transferred to a reactor for hydrothermal reaction. After the reaction is completed, a modifier is added to continue the reaction, and after purification, the rod-shaped boehmite is obtained.

2. The method for producing rod-shaped boehmite according to claim 1, characterized in that: The aluminum-containing substance is an aluminum salt.

3. The method for producing rod-shaped boehmite according to claim 2, characterized in that: The aluminum-containing salt includes one or more of aluminum chloride and aluminum nitrate.

4. The method for producing rod-shaped boehmite according to claim 1, characterized in that: The concentration is 0.02-0.16 mol·mL -1 .

5. The method for producing rod-shaped boehmite according to claim 1, characterized in that: The precipitant is an alkaline substance.

6. The method for producing rod-shaped boehmite according to claim 5, characterized in that: The alkaline substance includes one or more of hydrazine hydrate, ammonia water and sodium hydroxide.

7. The method for producing rod-shaped boehmite according to claim 1, characterized in that: The modifier is a carboxylic acid.

8. The method for producing rod-shaped boehmite according to claim 7, characterized in that: The carboxylic acid is an alkyl carboxylic acid.

9. The method for producing rod-shaped boehmite according to claim 1, characterized in that: The hydrothermal reaction conditions are 120-200° C., 12 h.