Regeneration method of aluminum salt for impurity removal of lithium salt solution
Through the steps of pickling, acid dissolution, alkalinization and water washing, the pH and concentration are controlled, and the re-lifeization problem of inactivated aluminum hydroxide is solved, the process is simplified, the cost is reduced, and the efficiency of lithium salt solution is improved. Recycling of resources is realized.
Patent Information
- Application Number
- CN202410954075.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the inactivated aluminum hydroxide is difficult to re-live, resulting in difficulty in comprehensive resource utilization, and the lithium salt solution has complex impurity removal process, high cost and low efficiency.
By using the steps of pickling, acid dissolution, alkalization and water washing, the impurities in aluminum hydroxide are washed away by controlling the pH and alkalinity and concentration, and their activity is restored to form a renewable active aluminum hydroxide colloid.
The process flow is simplified, production efficiency is improved, production costs are reduced, and the recycling and comprehensive utilization of resources is realized.
Smart Images

Figure CN118908259A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum salt regeneration, and more specifically to a method for regenerating aluminum salt for removing impurities from a lithium salt solution. Background Art
[0002] Salt lake lithium resources are an important strategic resource. Especially in the context of the rapid development of new energy vehicles and energy storage, their development and utilization have received widespread attention. China's salt lake lithium resources are mainly distributed in the salt lakes of the Qinghai-Tibet Plateau, of which Qinghai Salt Lake lithium resources account for about 80% of the country's total lithium resources, of which Qinghai Salt Lake lithium resources account for nearly 50%. Although salt lake lithium resources are abundant, their development faces a series of technical challenges. For example, the green and low-cost separation of magnesium and lithium from high magnesium-lithium ratio salt lake brine is a global problem, and it is also the key to the salt lake lithium extraction process and the bottleneck of comprehensive resource utilization. In addition, there are bottlenecks in the exploration technology, mining technology and processing technology of salt lake lithium resources to varying degrees, such as immature exploration technology, low mining efficiency, high cost, and severe environmental pollution.
[0003] Under the background of energy conservation, emission reduction, low carbon and environmental protection, the vigorous development of lithium battery new energy industry has driven the development of lithium resources in salt lakes. Aluminum salts are gradually being developed for lithium extraction and impurity removal in salt lakes due to their highly selective adsorption of lithium ions. Lithium extraction by aluminum salt adsorption is a commonly used lithium resource development technology, which uses the highly selective adsorption of aluminum salts on lithium ions to separate lithium from the solution.
[0004] At present, our company has synthesized an active aluminum hydroxide colloid for the removal of impurities in lithium bicarbonate solution. The active aluminum hydroxide can adsorb impurities such as magnesium, calcium, and fluorine. When the adsorption load is saturated, the aluminum hydroxide will lose its activity. How to regenerate and activate the inactivated aluminum hydroxide to achieve comprehensive resource utilization has become a major problem.
[0005] Therefore, how to achieve the regeneration and activation of deactivated aluminum hydroxide has become an urgent problem to be solved. Based on the above background, the present invention proposes a regeneration method of aluminum salt for removing impurities from lithium salt solution. Summary of the invention
[0006] The object of the present invention is to provide a method for regenerating aluminum salt for removing impurities from lithium salt solution, aiming at the problems in the prior art, simplifying the process, reducing costs and improving production efficiency.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A method for regenerating an aluminum salt for removing impurities from a lithium salt solution comprises the following steps:
[0009] S1. Acid washing: add water to the deactivated aluminum hydroxide for pulping, add hydrochloric acid or sulfuric acid for acid washing, wash away lithium, fluorine, magnesium, calcium and other elements in the deactivated aluminum hydroxide, and then filter press;
[0010] S2, acid dissolution: After acid washing in S1, add water to the aluminum hydroxide to make a pulp, add hydrochloric acid or sulfuric acid to dissolve it, and obtain an aluminum salt solution;
[0011] S3, alkalization: adding liquid alkali to the aluminum salt solution obtained in S2 to neutralize and precipitate aluminum to obtain aluminum hydroxide;
[0012] S4, water washing: add water to the aluminum hydroxide obtained in S3, slurry it and wash it with water to obtain active aluminum hydroxide after desorption of impurities.
[0013] Preferably, the solid-liquid ratio of pulping in step S1 is 1:3, and the pH value of acidification by adding hydrochloric acid or sulfuric acid is 4-5, in order to control the appropriate amount of acid to wash away lithium, fluorine, magnesium, calcium and other elements in the inactivated aluminum hydroxide, and the aluminum hydroxide is not dissolved by the acid at this pH value.
[0014] Preferably, in step S2, the solid-liquid ratio of pulping is 1:3, and the pH value of acidification by adding hydrochloric acid or sulfuric acid is 2-3, in order to control the appropriate amount of acid to dissolve the aluminum hydroxide after pickling.
[0015] Preferably, in step S3, a 30% sodium hydroxide solution is added until the pH value of the solution is 5-6 in order to control the appropriate amount of acid to precipitate aluminum to generate active aluminum hydroxide.
[0016] Preferably, the water washing solid-liquid ratio in step S4 is 1:3, in order to wash away the sodium salt in the regenerated active aluminum hydroxide.
[0017] Technical effects and advantages of the present invention:
[0018] The present invention provides a regeneration method for aluminum salt used for removing impurities from lithium salt solution with respect to active aluminum hydroxide colloid used for removing impurities from lithium salt solution, controls an appropriate amount of acid so that aluminum hydroxide is not dissolved, washes away impurities adsorbed by aluminum hydroxide, and improves production efficiency; and restores the activity of aluminum hydroxide colloid through acid dissolution and alkalization so that it can be continuously used, simplifies the process flow, improves production efficiency, reduces production cost, and realizes the recycling and comprehensive utilization of resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention is a flow chart of a method for regenerating aluminum salt for removing impurities from lithium salt solution. DETAILED DESCRIPTION
[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0021] The main components of the deactivated aluminum hydroxide colloid used are shown in the following table: (unit: ppm).
[0022] Al Li F Mg Ca 27376.279 12905.386 985.32 696.226 85.510
[0023] Example 1
[0024] This embodiment provides a method for regenerating aluminum salt for removing impurities from a lithium salt solution, comprising the following steps:
[0025] S1. Pickling: Add water to the deactivated aluminum hydroxide, slurry at a solid-liquid ratio of 1:2, add hydrochloric acid to adjust the pH value to 5, stir for 30 minutes and filter press;
[0026] S2, acid dissolution: add water to the acid-washed aluminum hydroxide in S1, slurry it at a solid-liquid ratio of 1:2, and add hydrochloric acid to adjust the pH value to 3;
[0027] S3, alkalization: add 30% sodium hydroxide solution to the solution obtained in S2 until the pH value is 6, and filter press after 30 minutes;
[0028] S4, water washing: add pure water to the filter cake obtained in S3, beat with water at a ratio of 1:3, and filter press after 30 minutes to obtain active aluminum hydroxide colloid. The test results are shown in the following table: (unit: ppm)
[0029] Al Li F Mg Ca 47558.410 4264.556 78.886 62.911 7.975
[0030] Example 2
[0031] This embodiment provides a method for regenerating aluminum salt for removing impurities from a lithium salt solution, comprising the following steps:
[0032] S1. Pickling: Add water to the deactivated aluminum hydroxide, slurry at a solid-liquid ratio of 1:3, add hydrochloric acid to adjust the pH value to 4.5, stir for 30 minutes and filter press;
[0033] S2, acid dissolution: add water to the acid-washed aluminum hydroxide in S1, slurry it at a solid-liquid ratio of 1:3, and add hydrochloric acid to adjust the pH value to 2;
[0034] S3, alkalization: add 30% sodium hydroxide solution to the solution obtained in S2 until the pH value is 5.5, and filter press after 30 minutes;
[0035] S4, water washing: add pure water to the filter cake obtained in S3, beat with water at a ratio of 1:3, and filter press after 30 minutes to obtain active aluminum hydroxide colloid. The test results are shown in the following table: (unit: ppm)
[0036] Al Li F Mg Ca 57799.546 4948.391 79.996 24.262 2.276
[0037] Example 3
[0038] This embodiment provides a method for regenerating aluminum salt for removing impurities from a lithium salt solution, comprising the following steps:
[0039] S1. Pickling: Add water to the deactivated aluminum hydroxide, slurry at a solid-liquid ratio of 1:3, add sulfuric acid to adjust the pH value to 4, stir for 30 minutes and filter press;
[0040] S2, acid dissolution: add water to the acid-washed aluminum hydroxide in S1, slurry it at a solid-liquid ratio of 1:3, and add sulfuric acid to adjust the pH value to 2.5;
[0041] S3, alkalization: add 30% sodium hydroxide solution to the solution obtained in S2 until the pH value is 5, and filter press after 30 minutes;
[0042] S4, water washing: add pure water to the filter cake obtained in S3, beat with water at a ratio of 1:3, and filter press after 30 minutes to obtain active aluminum hydroxide colloid. The test results are shown in the following table: (unit: ppm)
[0043] Al Li F Mg Ca 55731.770 3777.823 55.655 12.623 8.077
[0044] It can be seen from the above test data that the method provided by the present invention can efficiently desorb impurities adsorbed by aluminum hydroxide colloid, thereby restoring activity, simplifying the process flow, improving production efficiency, reducing production costs, and realizing comprehensive recycling of resources.
[0045] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for regenerating aluminum salt for removing impurities from lithium salt solution, characterized in that: The following steps are involved: S1. Acid washing: add water to the deactivated aluminum hydroxide for pulping, add hydrochloric acid or sulfuric acid for acid washing, wash away lithium, fluorine, magnesium, calcium and other elements in the deactivated aluminum hydroxide, and then filter press; S2, acid dissolution: After acid washing in S1, add water to the aluminum hydroxide to make a pulp, add hydrochloric acid or sulfuric acid to dissolve it, and obtain an aluminum salt solution; S3, alkalization: adding liquid alkali to the aluminum salt solution obtained in S2 to neutralize and precipitate aluminum to obtain aluminum hydroxide; S4, water washing: add water to the aluminum hydroxide obtained in S3, slurry it and wash it with water to obtain active aluminum hydroxide after desorption of impurities.
2. The method for regenerating aluminum salt for removing impurities from lithium salt solution according to claim 1, characterized in that: In step S1, the solid-liquid ratio of pulping is 1:3, the pH value of acidification is 4-5, and the pickling time is 30 minutes.
3. The method for regenerating aluminum salt for removing impurities from lithium salt solution according to claim 1, characterized in that: In step S2, the solid-liquid ratio of pulping is 1:3, and the pH value of acid dissolution is 1.5-2.
5.
4. The method for regenerating aluminum salt for removing impurities from lithium salt solution according to claim 1, characterized in that: In step S3, a sodium hydroxide solution with a concentration of 30% is added, and the pH value of the neutralization is 5-6.