Barium titanate material doped with rare earth elements and preparation method thereof

By doping rare earth elements into barium titanate material and using nano nickel powder in the modified solution for gel-sintering treatment, the problem of poor dielectric performance of barium titanate material is solved, and low dielectric loss and stable temperature are achieved Good effect.

CN118908272APending Publication Date: 2024-11-08CHANGDI NEW MATERIAL TECHNOLOGY (SHANGHAI) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411009132.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing barium titanate materials have poor dielectric performance in MLCC, high dielectric loss and poor temperature stability, making it difficult to meet the high performance needs of miniaturized electronic devices.

Method used

The preparation method of barium titanate material doped with rare earth elements is adopted. The rare earth elements are doped by co-precipitation method, combined with the nano nickel powder and regulator in the modified liquid, and the gel-sintering treatment is carried out to regulate the temperature and molar ratio, and optimize the material. microstructure and crystal structure reduce dielectric loss and improve temperature stability.

Benefits of technology

The dielectric loss of barium titanate material is significantly reduced and its temperature stability is improved. The resulting material has excellent dielectric properties and microstructure uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908272A_ABST
    Figure CN118908272A_ABST
Patent Text Reader

Abstract

The invention relates to the field of barium titanate materials, and particularly discloses a rare earth element-doped barium titanate material and a preparation method thereof, and the preparation method comprises the following steps: step 1, uniformly mixing a barium chloride solution and a titanium tetrachloride solution to obtain a mixed solution; step 2, adding an oxalic acid solution containing rare earth elements into the mixed solution to obtain a precipitation product, uniformly dispersing the precipitation product into the modified solution, heating to 60-85 DEG C, stirring to form a gel precursor, and carrying out pre-roasting and high-temperature sintering treatment on the obtained gel precursor to obtain a barium titanate material; the oxalic acid solution containing the rare earth elements comprises an oxalic acid solution, rare earth oxide and a dispersing agent, the modification liquid comprises a binder, a regulator and nano nickel powder; the molar ratio of the barium element to the titanium element to the rare earth element is 1: (1-1.5): (0.01-0.1). The obtained barium titanate material has the advantages of low dielectric loss and good temperature stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of barium titanate materials, and more specifically, to a barium titanate material doped with a rare earth element and a preparation method thereof. Background Art

[0002] With the development of the semiconductor industry, the requirements for electronic components are becoming more and more stringent. Barium titanate materials are widely used in electronic devices, sensors, capacitors and other fields. Among them, barium titanate materials are most widely used in MLCC. With the development trend of miniaturization and micro-miniaturization of MLCC, higher performance barium titanate powder is urgently needed.

[0003] At present, there are many methods for preparing barium titanate. Among them, the high-temperature synthesis method uses barium carbonate and titanium dioxide as raw materials and reacts and synthesizes them at 1200℃-1250℃. Although the raw materials of this method are cheap and easy to obtain, the dielectric properties of the obtained barium titanate material are poor, the dielectric loss is high and the temperature stability is poor. Summary of the invention

[0004] In order to improve the dielectric properties of barium titanate materials so that the barium titanate materials have the advantages of low dielectric loss and good temperature stability, the present application provides a barium titanate material doped with a rare earth element and a preparation method thereof.

[0005] In the first aspect, the present application provides a barium titanate material doped with a rare earth element using the following technical solution: A method for preparing a barium titanate material doped with a rare earth element comprises the following steps: Step 1, mixing the barium chloride solution and the titanium tetrachloride solution uniformly to obtain a mixed solution; Step 2, adding an oxalic acid solution containing a rare earth element to the mixed solution to obtain a precipitated product, uniformly dispersing the precipitated product into the modified solution, heating to 60-85° C. and stirring to form a gel precursor, and pre-calcining and high-temperature sintering the obtained gel precursor to obtain a barium titanate material; The oxalic acid solution containing rare earth elements comprises oxalic acid solution, rare earth oxide and dispersant; The modified liquid comprises a binder, a regulator and nano nickel powder; The molar ratio of the barium element to the titanium element to the rare earth element is 1:(1-1.5):(0.01-0.1).

[0006] By adopting the above technical scheme, the present application adopts a co-precipitation method to obtain a precipitated product, dopes rare earth elements, refines the material grains, and modifies them through a modifying liquid to enhance the chemical uniformity of the multi-component system, control the temperature and precisely regulate the gelation temperature, and combine the volatilization process of the control regulator to obtain barium titanate particles with good structural uniformity based on a gel-sintering treatment process, thereby reducing the dielectric loss of the barium titanate material and improving its temperature stability.

[0007] The molar ratio of barium to titanium to rare earth elements is controlled, and the uniform dispersion of each raw material component is promoted by dispersants, and rare earth elements are doped into the product to adjust the internal microscopic properties of the material. The nickel powder can be effectively attached to the surface of the precipitated product through a binder. The regulator can further assist in dissolution, adjust the viscosity and fluidity of the system, and has good volatility, which helps the uniform adhesion between components. The crystalline state of the material can be further regulated in the pre-baking stage, and then high-temperature sintering treatment is carried out. The nano nickel powder in the modified solution can further improve the sintering shrinkage performance of the material, thereby obtaining a barium titanate material with uniform microstructure.

[0008] Preferably, the pre-sintering conditions are as follows: heating to 200-400°C at a rate of 3-5°C / min and keeping warm for 1-2h; the high temperature sintering conditions are as follows: raising the temperature to 750-950°C and keeping warm for 2-3h.

[0009] By adopting the above technical solution, the temperature can be controlled in sections, which helps to adjust the microscopic morphology of the material and thus improve the overall performance of the product.

[0010] Preferably, the oxalic acid solution containing rare earth elements comprises the following raw materials in parts by weight: 70-90 parts of oxalic acid solution, 1-4 parts of rare earth oxide, and 1-3 parts of dispersant.

[0011] Preferably, the modified solution comprises the following raw materials in parts by weight: 10-20 parts of a binder, 10-30 parts of a regulator and 3-6 parts of nano nickel powder.

[0012] Furthermore, the particle size of the nano nickel powder is 100-500nm.

[0013] By adopting the above technical solution, the component dosage of the oxalic acid solution containing rare earth elements and the modified liquid is optimized, which is conducive to doping rare earth elements, assisting in improving the grain and crystalline state of the material, reducing the dielectric loss of the material and improving its temperature stability.

[0014] Preferably, the dispersant is Walker VOK-41000 dispersant or BYK-108 dispersant.

[0015] Preferably, the rare earth oxide includes one or more of lanthanum oxide, yttrium oxide, and cerium oxide.

[0016] By adopting the above technical solution, suitable rare earth oxides are selected to provide corresponding rare earth elements, thereby regulating the crystal structure and electron distribution of barium titanate to improve its electrical properties.

[0017] Preferably, the binder comprises polyvinyl butyral and ethyl cellulose in a mass ratio of (4-8):1.

[0018] Preferably, the regulator is one or more of terpineol, isoborneol acetate, isophorone, and butyl acetate.

[0019] Preferably, the regulator is obtained by uniformly mixing terpineol, isoborneol acetate and butyl acetate in a mass ratio of (1-2):(1.5-3):1.

[0020] In a second aspect, the present application provides a barium titanate material doped with a rare earth element, using the following technical solution: a barium titanate material doped with a rare earth element, prepared by the above-mentioned method for preparing a barium titanate material doped with a rare earth element.

[0021] By adopting the above technical solution, the obtained barium titanate material has excellent quality, low dielectric loss and good temperature stability.

[0022] In summary, this application has the following beneficial effects: 1. By adjusting the molar ratio of barium to titanium to rare earth elements, using a dispersant to promote uniform dispersion of each raw material component, and doping the product with rare earth elements, the internal microscopic properties of the material are adjusted, and the nickel powder is effectively attached to the surface of the precipitated product through a binder. The regulator can further assist in dissolution, adjust the viscosity and fluidity of the system, and has good volatility, which is conducive to uniform adhesion between components. The crystalline state of the material can be further regulated in the pre-baking stage, and then high-temperature sintering treatment is carried out. The nano nickel powder in the modified solution can further improve the sintering shrinkage performance of the material, thereby obtaining a barium titanate material with uniform microstructure.

[0023] 2. Doping rare earth elements, refining the material grains, and modifying them through modifying liquid to improve the chemical uniformity of the multi-component system, control the temperature and accurately regulate the gelation temperature, combine the volatilization process of the control regulator, and obtain barium titanate particles with good structural uniformity based on the gel-sintering process, thereby reducing the dielectric loss of the barium titanate material and improving its temperature stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the SEM image of the barium titanate material of Example 8 of the present application.

[0025] Figure 2This is the SEM image of the barium titanate material of Comparative Example 1 of the present application.

[0026] Figure 3 This is the SEM image of the barium titanate material of Comparative Example 2 of the present application.

[0027] Figure 4 This is the SEM image of the barium titanate material of Comparative Example 3 of the present application.

[0028] Figure 5 This is the SEM image of the barium titanate material of Comparative Example 4 of the present application. DETAILED DESCRIPTION

[0029] The embodiments of the present invention will be described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially. Example

[0030] Example 1 A method for preparing a barium titanate material doped with a rare earth element comprises the following steps: Step 1, mixing the barium chloride solution and the titanium tetrachloride solution uniformly to obtain a mixed solution; Step 2, adding an oxalic acid solution containing a rare earth element to the mixed solution to obtain a precipitated product, uniformly dispersing the precipitated product into the modified solution, heating to 60°C and stirring to form a gel precursor, and pre-calcining and high-temperature sintering the obtained gel precursor. The pre-calcination conditions are specifically: heating to 400°C at a rate of 3-5°C / min and keeping warm for 1h; the high-temperature sintering conditions are specifically: raising the temperature to 750°C at a rate of 5-8°C / min and keeping warm for 3h to obtain a barium titanate material; The oxalic acid solution containing rare earth elements includes 7kg of oxalic acid solution with a mass concentration of 10%, 0.1kg of lanthanum oxide and 0.1kg of dispersant; the modified liquid includes 1kg of binder, 3kg of regulator and 0.3kg of nano nickel powder, and the particle size of the nano nickel powder is 100-150nm; The molar ratio of barium to titanium to rare earth elements is 1:1.5:0.1; The dispersant is Walker VOK-41000 dispersant, the binder is polyvinyl butyral and ethyl cellulose in a mass ratio of 4:1, the model of polyvinyl butyral is B79, and the CAS number of ethyl cellulose is 9004-57-3; the regulator is pinene alcohol and isoborneol acetate in a mass ratio of 2:1, the CAS number of pinene alcohol is 8000-41-7, and the CAS number of isoborneol acetate is 125-12-2.

[0031] Example 2 A method for preparing a barium titanate material doped with a rare earth element comprises the following steps: Step 1, mixing the barium chloride solution and the titanium tetrachloride solution uniformly to obtain a mixed solution; Step 2, adding an oxalic acid solution containing a rare earth element to the mixed solution to obtain a precipitated product, uniformly dispersing the precipitated product into the modified solution, heating to 85°C and stirring to form a gel precursor, and pre-calcining and high-temperature sintering the obtained gel precursor. The pre-calcination conditions are specifically: heating to 200°C at a rate of 3-5°C / min and keeping warm for 2h; the high-temperature sintering conditions are specifically: raising the temperature to 950°C at a rate of 5-8°C / min and keeping warm for 2h to obtain a barium titanate material; The oxalic acid solution containing rare earth elements includes 9 kg of oxalic acid solution with a mass concentration of 10%, 0.4 kg of yttrium oxide and 0.3 kg of dispersant; the modified liquid includes 2 kg of binder, 1 kg of regulator and 0.6 kg of nano nickel powder, and the particle size of the nano nickel powder is 400-500 nm; The molar ratio of barium to titanium to rare earth elements is 1:1.2:0.01; The dispersant is BYK-108 dispersant, the binder is ethyl cellulose, and the regulator is isophorone and butyl acetate in a mass ratio of 3:1. The CAS number of isophorone is 78-59-1, and the CAS number of butyl acetate is 123-86-4.

[0032] Example 3 The difference from Example 1 is that, in step 2, an oxalic acid solution containing rare earth elements is added to the mixed solution to obtain a precipitated product, the precipitated product is evenly dispersed in the modified solution, heated to 75°C and stirred to form a gel precursor, and the obtained gel precursor is pre-calcined and high-temperature sintered, and the pre-calcination conditions are specifically: heating to 300°C at a rate of 3-5°C / min, and keeping warm for 1.2h; the high-temperature sintering conditions are specifically: raising the temperature to 905°C at a rate of 5-8°C / min, keeping warm for 2.5h, to obtain a barium titanate material; wherein the molar ratio of barium element to titanium element to rare earth element is 1:1:0.07; the rest is the same as Example 1.

[0033] Example 4 The difference from Example 3 is that the oxalic acid solution containing rare earth elements includes 8 kg of oxalic acid solution with a mass concentration of 10%, 0.2 kg of lanthanum oxide, 0.2 kg of cerium trioxide and 0.3 kg of dispersant; the dispersant is BYK-108 dispersant; and the rest is the same as Example 3.

[0034] Example 5 The difference from Example 4 is that the modified liquid includes 3 kg of binder, 1 kg of regulator and 0.2 kg of nano nickel powder, the binder is polyvinyl butyral ester, the regulator is isoborneol acetate, and the rest is the same as Example 4.

[0035] Example 6 The difference from Example 4 is that the modified liquid includes 1.2 kg of binder, 2.1 kg of regulator and 0.45 kg of nano nickel powder, and the particle size of the nano nickel powder is 200-240 nm; the rest is the same as Example 4.

[0036] Example 7 The difference from Example 6 is that the binder is polyvinyl butyral ester and ethyl cellulose in a mass ratio of 5.8:1, and the rest is the same as Example 6.

[0037] Example 8 The difference from Example 6 is that the regulator is terpineol, isoborneol acetate and butyl acetate mixed in a mass ratio of 1:2:1, and the rest is the same as Example 6.

[0038] Example 9 The difference from Example 8 is that the regulator is obtained by uniformly mixing terpineol, isoborneol acetate and butyl acetate in a mass ratio of 3:1:0.7, and the rest is the same as Example 8.

[0039] Comparative Example Comparative Example 1 The difference from Example 8 is that the molar ratio of barium element to titanium element to rare earth element is 1:0.5:0.003, and the rest is the same as Example 8.

[0040] Comparative Example 2 The difference from Example 8 is that, in step 2, an oxalic acid solution containing rare earth elements is added to the mixed solution to obtain a precipitated product, the precipitated product is evenly dispersed in the modified liquid, stirred evenly at room temperature, and sintered at 900°C for 2.5h to obtain a barium titanate material; the rest is the same as Example 8.

[0041] Comparative Example 3 The difference from Example 8 is that the oxalic acid solution containing rare earth elements includes 10 kg of oxalic acid solution with a mass concentration of 10% and 0.2 kg of cerium trioxide, and the rest is the same as Example 8.

[0042] Comparative Example 4 The difference from Example 8 is that the modified liquid includes 2 kg of silane coupling agent and 0.3 kg of nano nickel powder, and the rest is the same as Example 8.

[0043] Performance testing The dielectric loss DF and temperature stability TCC performance tests were performed on Examples 1-9 and Comparative Examples 1-4 according to Sections 4.5.1, 4.5.2 and 4.6 of GB / T 21042-2007 “Fixed Capacitors for Electronic Equipment”, and the results are recorded in Table 1.

[0044] Table 1 It can be seen from Examples 1-8 and Table 1 that the barium titanate material obtained by the preparation method of the present application has the advantages of low dielectric loss and good temperature stability, and the product performance is good. Figure 1 It can be seen that the microstructure of barium titanate material is uniform.

[0045] Combining Example 8 and Comparative Examples 1-4, it can be seen that in Comparative Example 1, the molar ratio of barium element to titanium element to rare earth element is unbalanced, in Comparative Example 2, the raw materials of each component are mixed and stirred evenly and then sintered directly, in Comparative Example 3, the components of the oxalic acid solution containing rare earth elements and the amounts of the corresponding components are adjusted; in Comparative Example 4, the components and amounts of the modified liquid are adjusted, and the barium titanate materials obtained in Comparative Examples 1-4 have high dielectric loss and poor temperature stability.

[0046] By comparison Figure 1 as well as Figure 2-5 It can be seen that the barium titanate material prepared in Example 8 has a uniform microstructure, while the barium titanate materials obtained in Comparative Examples 1-4 have poor microstructures, with agglomeration, uneven phase distribution, uneven grain size distribution, and crystal defects in the material.

[0047] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A method for preparing a barium titanate material doped with a rare earth element, characterized in that: The following steps are involved: Step 1, mixing the barium chloride solution and the titanium tetrachloride solution uniformly to obtain a mixed solution; Step 2, adding an oxalic acid solution containing a rare earth element to the mixed solution to obtain a precipitated product, uniformly dispersing the precipitated product into the modified solution, heating to 60-85° C. and stirring to form a gel precursor, and pre-calcining and high-temperature sintering the obtained gel precursor to obtain a barium titanate material; The oxalic acid solution containing rare earth elements comprises oxalic acid solution, rare earth oxide and dispersant; The modified liquid comprises a binder, a regulator and nano nickel powder; The molar ratio of the barium element to the titanium element to the rare earth element is 1:(1-1.5):(0.01-0.1); The binder includes polyvinyl butyral ester and ethyl cellulose in a mass ratio of (4-8):

1.

2. The method for preparing the barium titanate material doped with rare earth elements according to claim 1, characterized in that: The pre-sintering conditions are as follows: heating to 200-400°C at a rate of 3-5°C / min and keeping the temperature for 1-2h; the high-temperature sintering conditions are as follows: heating to 750-950°C and keeping the temperature for 2-3h.

3. The method for preparing the barium titanate material doped with rare earth elements according to claim 1, characterized in that: The oxalic acid solution containing rare earth elements comprises the following raw materials in parts by weight: 70-90 parts of oxalic acid solution, 1-4 parts of rare earth oxide, and 1-3 parts of dispersant.

4. The method for preparing the barium titanate material doped with rare earth elements according to claim 1, characterized in that: The modified liquid comprises the following raw materials in parts by weight: 10-20 parts of a binder, 10-30 parts of a regulator and 3-6 parts of nano nickel powder.

5. The method for preparing the barium titanate material doped with rare earth elements according to claim 1, characterized in that: The dispersant is Walker VOK-41000 dispersant or BYK-108 dispersant.

6. The method for preparing the barium titanate material doped with rare earth elements according to claim 3, characterized in that: The rare earth oxide includes one or more of lanthanum oxide, yttrium oxide and cerium oxide.

7. The method for preparing the barium titanate material doped with rare earth elements according to claim 1, characterized in that: The regulator is one or more of terpineol, isoborneol acetate, isophorone and butyl acetate.

8. The method for preparing the barium titanate material doped with rare earth elements according to claim 8, characterized in that: The regulator is obtained by uniformly mixing terpineol, isoborneol acetate and butyl acetate in a mass ratio of (1-2): (1.5-3):

1.

9. A barium titanate material doped with a rare earth element, characterized in that: The barium titanate material doped with rare earth elements is prepared by the preparation method of any one of claims 1 to 9.

Citation Information

Cited By

  • Preparation method of high-performance modified barium titanate

    CN120794647A