Method for preparing high-purity manganous-manganic oxide through segmented roasting method

Through the segmented roasting method, high-purity trimanium tetraoxide is prepared by soluble manganese salt, which solves the problems of high raw material costs and complex process, and realizes the preparation of trimanium tetraoxide with high purity and uniform particle size, which is suitable for lithium battery positive electrode materials. Simple process, high safety and low cost.

CN118908283APending Publication Date: 2024-11-08浙江格派钴业新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411311572.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When preparing high-purity manganese tetraoxide, the raw materials are costly, complex processes, and difficult to control the degree of oxidation. The generated products are prone to clustered particles, limiting the application of the lithium battery industry.

Method used

The soluble manganese salt is first dissolved in water, and the powder is obtained by spray-drying, and the high-temperature calcination is used to form a trimanganese tetraoxide precursor. Then, the low-temperature calcination is carried out under a reducing atmosphere, combining pickling, crushing, washing, Drying treatment to control grain size and particle size distribution.

Benefits of technology

It has achieved high purity, low impurity, and uniform particle size distribution of trimanium tetraoxide. It has simple process, high safety and low cost, and is suitable for the preparation of lithium battery positive electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908283A_ABST
    Figure CN118908283A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high-purity manganous-manganic oxide, in particular to a method for preparing high-purity manganous-manganic oxide through a segmented roasting method. The method is simple in operation steps, soluble manganese salt is used as a raw material, the soluble manganese salt is dissolved in pure water and then subjected to spray drying to prepare powder, and the powder is subjected to high-temperature roasting in an air or oxygen atmosphere by using a muffle furnace to prepare a manganous-manganic oxide precursor; and placing the cooled and crushed precursor in a tubular furnace, roasting in a reducing gas atmosphere at a low temperature to obtain a manganous-manganic oxide crude product, and carrying out acid pickling, crushing, washing and drying treatment on the crude product to prepare the high-purity manganous-manganic oxide. Mn in the manganous-manganic oxide prepared by the method is more than 70%, and the manganous-manganic oxide is low in impurity content, uniform in particle size distribution, high in consistency and good in activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-purity trimanganese tetraoxide, in particular to a method for preparing high-purity trimanganese tetraoxide by a staged roasting method. Background Art

[0002] Manganese manganate tetroxide, a key raw material in the industrial production of manganese-zinc ferrite materials, is widely used in the production of electronic components, sensors, and electromagnetic compatibility. Furthermore, manganese manganate tetroxide has a wide range of applications. For example, nano-manganese manganate tetroxide can act as a catalyst to promote the decomposition of methane, carbon, and nitrogen oxides, as well as the selective reduction of nitrobenzene. High-purity manganese manganate tetroxide is also used in thermistors, semiconductor ceramics, paints, and coatings. With the rapid rise of the new energy industry in recent years, demand for manganese manganate in lithium-ion batteries has surged, primarily for use in the preparation of manganese-based cathode materials such as lithium manganate, lithium nickel manganate, and lithium manganese phosphate. Compared to the demands of traditional industries, the cathode materials industry places even stricter requirements on the purity and quality of manganese manganate, encompassing a number of indicators such as purity, impurity content, particle size distribution, morphology, crystal form, and apparent density.

[0003] Common methods for producing manganese tetraoxide in current industrial production include the metallic manganese method, the manganese salt method, and the roasting method. The metallic manganese method involves directly pulverizing electrolytic manganese flakes to form a suspension, adding an appropriate amount of catalyst, and introducing oxygen or air to catalytically oxidize the manganese slurry. The crude manganese tetraoxide is then stirred, washed, filtered, and dried to obtain the final product. This method, also known as the electrolytic manganese suspension oxidation method, is simple, easy to operate, and offers high yields, high manganese recovery rates, and high product purity. However, the high cost of raw materials, particularly with the rising price of electrolytic manganese flakes, severely limits this method's market competitiveness and poor risk tolerance. The manganese salt method uses manganese salts such as manganese sulfate, manganese chloride, and manganese nitrate as raw materials. By adding an alkaline solution such as liquid caustic soda or ammonia, the divalent manganese ions in the solution are precipitated as manganese hydroxide or other manganese compounds. The precipitate is then oxidized to manganese tetraoxide using an oxidizing agent, and the product is then washed and treated to remove impurities. The Chinese invention patent publication number CN1935673A describes a method of directly oxidizing free divalent manganese ions in the solution to produce trimanganese tetraoxide using manganese sulfate or manganese chloride solution as raw materials, adding ammonia water as a neutralizing agent, and controlling the pH change rate during the reaction process with oxygen or air as an oxidant. This method is simple in steps, has low operational difficulty, a wide range of raw material sources, low cost, and mild reaction conditions. A trimanganese tetraoxide product with good activity can be prepared by rationally regulating process parameters. However, it also has disadvantages such as low conversion efficiency, low recovery rate, difficulty in controlling the reaction degree and oxidation time, and easy overoxidation. The roasting method involves roasting metallic manganese or manganese oxides, hydroxides, sulfates, sulfites, carbonates, nitrates, and permanganates at high temperatures in air, followed by cooling and pulverization to produce trimanganese tetraoxide. Chinese invention patent publication number CN115286041A discloses a method for preparing high-purity manganese tetraoxide by subjecting a manganese salt to a primary roasting process, followed by cooling, crushing, dissolving in concentrated sulfuric acid, purification, and impurity removal, followed by precipitation and oxidation with alkali, and a secondary roasting process. This method innovatively proposes feeding oxygen generated when manganese tetraoxide is dissolved in concentrated sulfuric acid into a roasting furnace, and using carbon dioxide generated by carbon combustion to purify and remove impurities from the manganese sulfate solution. However, the reaction process is complex, requiring multiple oxidation steps to produce manganese tetraoxide, making the degree of oxidation difficult to control. Furthermore, the manganese tetraoxide prepared by this method tends to form clustered particles, limiting its application in the lithium battery industry.

[0004] Therefore, how to use a widely available and inexpensive manganese source through a safe, simple, and easily controlled reaction process to prepare manganese tetraoxide with low impurity content, uniform particle size distribution, and high activity is the current technical difficulty. Summary of the Invention

[0005] In view of the shortcomings of the above-mentioned technologies, the present invention provides a staged roasting method for preparing high-purity manganese tetraoxide. The manganese tetraoxide prepared by this method has the characteristics of high purity, low impurities, uniform particle size distribution, and good morphology.

[0006] In order to achieve the above object, the present invention provides a method for preparing high-purity manganese tetraoxide by a staged roasting method, which comprises the following steps:

[0007] Step 1: Dissolve a soluble manganese salt with high purity and low impurity content in pure water and stir evenly to prepare a manganese salt solution.

[0008] Step 2: The manganese solution prepared in step 1 is prepared into manganese salt powder by a spray dryer.

[0009] Step 3: Take an appropriate amount of the powder prepared in step 2 and place it in a muffle furnace and calcine it at a high temperature in air or oxygen atmosphere;

[0010] Step 4: Cool and crush the trimanganese tetraoxide precursor prepared in step 3, and then place it in a tube furnace for calcination under a reducing gas atmosphere.

[0011] Step 5: pickling, crushing, washing and drying the manganese manganese oxide prepared in step 4.

[0012] The soluble manganese salt used in step 1 is at least one of manganese chloride, acetate, sulfate or nitrate.

[0013] The manganese concentration in the manganese solution prepared in step 1 is 40 g / L-150 g / L.

[0014] The calcination temperature in step 3 is 200° C.-1000° C. Preferably, the calcination temperature in step 3 is 400° C.-600° C.

[0015] The calcination time in step 3 is 2h-12h. Preferably, the calcination time in step 3 is 6h-8h.

[0016] The calcination temperature used in step 4 is 100° C.-700° C. Preferably, the calcination temperature used in step 4 is 200° C.-400° C.

[0017] The calcination time used in step 4 is 2h-6h.

[0018] The reducing gas used in step 4 is one of hydrogen, carbon monoxide and methane.

[0019] The present invention has simple operating steps. A soluble manganese salt with high purity and low impurity content is used as a raw material, and a powder is obtained by liquid spray drying. The powder is then subjected to high-temperature roasting in an air or oxygen atmosphere in a muffle furnace to obtain a trimanganese tetraoxide precursor. The cooled and crushed trimanganese tetraoxide precursor is then placed in a tube furnace and roasted at a lower temperature in a reducing gas atmosphere to obtain a crude trimanganese tetraoxide product. The crude product is then subjected to acid washing, crushing, washing, and drying to prepare high-purity trimanganese tetraoxide. The trimanganese tetraoxide prepared by this method has Mn content greater than 70%, low impurity content, uniform particle size distribution, high consistency, and high activity. The entire process is simple to operate, highly safe, and low in cost.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The present invention uses soluble manganese salt as raw material to roast into manganese tetraoxide. Compared with the traditional process using electrolytic manganese metal flakes as raw material, the raw material source is more extensive, stable and low in cost.

[0022] (2) The present invention can effectively control the grain size of trimanganese tetraoxide by controlling the roasting process and the roasting atmosphere, thereby obtaining trimanganese tetraoxide with good morphology, uniform particle size distribution and high consistency.

[0023] (3) The present invention effectively reduces the roasting temperature and time by adopting different roasting atmospheres, and provides a process flow with a simple process route, easy operation, low production cost, and large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Shown is a SEM image of trimanganese tetraoxide prepared in Example 5 of the present invention.

[0025] Figure 2 Shown is a SEM image of trimanganese tetraoxide prepared in Comparative Example 1 of the present invention.

[0026] Figure 3 Shown is the XRD pattern of trimanganese tetraoxide prepared in Example 5 of the present invention.

[0027] Figure 4 Shown is the XRD pattern of trimanganese tetraoxide prepared in Comparative Example 1 of the present invention.

[0028] Figure 5 The figure shows the process flow chart of preparing high-purity manganese manganese tetroxide by the staged roasting method of the present invention. DETAILED DESCRIPTION

[0029] In order to illustrate the present invention more clearly, the present invention is described in more comprehensive and detailed manner below in conjunction with the embodiments, but the protection scope of the present invention is not limited to the description.

[0030] Example 1

[0031] Step 1: Dissolve an appropriate amount of manganese sulfate in pure water and stir until completely dissolved to prepare a manganese solution with a Mn content of 60 g / L.

[0032] Step 2: The manganese solution prepared in step 1 is passed through a spray dryer to obtain manganese salt powder, with the inlet temperature set to 220°C and the outlet temperature set to 120°C.

[0033] Step 3: Place the powder prepared in step 2 in a muffle furnace and calcine it at 800°C in an air atmosphere for 4 hours;

[0034] Step 4: Cool and crush the trimanganese tetraoxide precursor obtained in step 3, place it in a tube furnace, and calcine it at 400° C. in a carbon monoxide atmosphere for 4 hours, and cool it in the furnace to obtain a crude trimanganese tetraoxide product.

[0035] Step 5: pickling, crushing, washing and drying the crude manganese tetraoxide product obtained in step 4.

[0036] Example 2

[0037] Step 1: Dissolve an appropriate amount of manganese sulfate in pure water and stir until completely dissolved to prepare a manganese solution with a Mn content of 120 g / L.

[0038] Step 2: The manganese solution prepared in step 1 is passed through a spray dryer to obtain manganese salt powder, with the inlet temperature set to 220°C and the outlet temperature set to 120°C.

[0039] Step 3: Place the powder prepared in step 2 in a muffle furnace and calcine at 400°C in an air atmosphere for 6 hours;

[0040] Step 4: Cool and crush the trimanganese tetraoxide precursor obtained in step 3, place it in a tube furnace, and calcine it at 700° C. in a carbon monoxide atmosphere for 3 hours, and cool it in the furnace to obtain a crude trimanganese tetraoxide product.

[0041] Step 5: pickling, crushing, washing and drying the crude manganese tetraoxide product obtained in step 4.

[0042] Example 3

[0043] Step 1: Dissolve an appropriate amount of manganese nitrate in pure water and stir until completely dissolved to prepare a manganese solution with a Mn content of 80 g / L.

[0044] Step 2: The manganese solution prepared in step 1 is passed through a spray dryer to obtain manganese salt powder, with the inlet temperature set to 220°C and the outlet temperature set to 120°C.

[0045] Step 3: Place the powder prepared in step 2 in a muffle furnace and calcine it at 500°C in an oxygen atmosphere for 10 hours;

[0046] Step 4: Cool and crush the trimanganese tetraoxide precursor obtained in step 3, place it in a tube furnace, and calcine it at 150° C. in a hydrogen atmosphere for 5 hours, and cool it in the furnace to obtain a crude trimanganese tetraoxide product.

[0047] Step 5: pickling, crushing, washing and drying the crude manganese tetraoxide product obtained in step 4.

[0048] Example 4

[0049] Step 1: Dissolve an appropriate amount of manganese chloride in pure water and stir until completely dissolved to prepare a manganese solution with a Mn content of 90 g / L.

[0050] Step 2: The manganese solution prepared in step 1 is passed through a spray dryer to obtain manganese salt powder, with the inlet temperature set to 220°C and the outlet temperature set to 120°C.

[0051] Step 3: Place the powder prepared in step 2 in a muffle furnace and calcine at 500°C in an air atmosphere for 8 hours;

[0052] Step 4: Cool and crush the trimanganese tetraoxide precursor obtained in step 3, place it in a tube furnace, and calcine it at 300° C. in a methane atmosphere for 3 hours, and cool it in the furnace to obtain a crude trimanganese tetraoxide product.

[0053] Step 5: pickling, crushing, washing and drying the crude manganese tetraoxide product obtained in step 4.

[0054] Example 5

[0055] Step 1: Dissolve an appropriate amount of manganese chloride in pure water and stir until completely dissolved to prepare a manganese solution with a Mn content of 110 g / L.

[0056] Step 2: The manganese solution prepared in step 1 is passed through a spray dryer to obtain manganese salt powder, with the inlet temperature set to 220°C and the outlet temperature set to 120°C.

[0057] Step 3: Place the powder prepared in step 2 in a muffle furnace and calcine it at 600°C in an oxygen atmosphere for 6 hours;

[0058] Step 4: Cool and crush the trimanganese tetraoxide precursor obtained in step 3, place it in a tube furnace, and calcine it at 250° C. in a methane atmosphere for 4 hours, and cool it in the furnace to obtain a crude trimanganese tetraoxide product.

[0059] Step 5: pickling, crushing, washing and drying the crude manganese tetraoxide product obtained in step 4.

[0060] The SEM and XRD patterns of the manganese tetraoxide product prepared in Example 5 are shown in Table 1. Figure 1 and Figure 3 .

[0061] Comparative Example 1

[0062] Step 1: Dissolve an appropriate amount of manganese chloride in pure water and stir until the manganese sulfate is completely dissolved to prepare a manganese solution with a Mn content of 90 g / L.

[0063] Step 2: The manganese solution prepared in step 1 is passed through a spray dryer to obtain manganese salt powder, with the inlet temperature set to 220°C and the outlet temperature set to 120°C.

[0064] Step 3: Place the powder prepared in step 2 in a muffle furnace and calcine at 600°C in an air atmosphere for 8 hours;

[0065] Step 4: Cool and crush the trimanganese tetraoxide precursor obtained in step 3, place it in a muffle furnace, and calcine it at 1000° C. in an air atmosphere for 5 hours, and cool it in the furnace to obtain a crude trimanganese tetraoxide product.

[0066] Step 5: pickling, crushing, washing and drying the crude manganese tetraoxide product obtained in step 4.

[0067] The SEM and XRD patterns of the manganese tetraoxide product prepared in Comparative Example 1 are shown in Figure 2 and Figure 4 .

[0068] The trimanganese tetraoxide products obtained in Examples 1 to 5 and Comparative Example 1 were tested for physical and chemical indicators, and the results are shown in Table 1. The results show that the trimanganese tetraoxide product prepared by the method of the present invention has the characteristics of high purity and low impurity element content.

[0069] The analysis and comparison of different experimental results are shown in Table 1.

[0070] Table 1 Analysis and comparison of different experimental results

[0071] experiment Mn% K% Na% Ca% Mg% Fe% Example 1 70.78 0.0079 0.016 0.040 0.037 0.0039 Example 2 70.63 0.0076 0.018 0.041 0.039 0.0038 Example 3 71.13 0.0077 0.015 0.038 0.037 0.0035 Example 4 71.25 0.0069 0.013 0.034 0.029 0.0034 Example 5 71.23 0.0072 0.012 0.032 0.035 0.0036 Comparative Example 1 68.43 0.0079 0.021 0.042 0.036 0.0038

[0072] In summary, referring to the data comparison in Table 1, it can be seen that when preparing high-purity manganese tetraoxide by the staged roasting method, the soluble manganese salt is first dissolved in water and sprayed to obtain a powder sample, and the powder sample is staged roasted at different roasting temperatures, times and atmospheres to obtain a manganese tetraoxide product with high purity and low impurity element content.

[0073] Compared with Comparative Example 1, the trimanganese tetraoxide prepared in Examples 1 to 5 has a higher Mn content and better product purity. Compared with Comparative Example 1, the trimanganese tetraoxide prepared in Example 5 has a more uniform grain size distribution, stronger characteristic peaks and fewer impurity peaks in the XRD analysis pattern, indicating that secondary calcination in a reducing gas atmosphere can effectively control the nucleation process of trimanganese tetraoxide, greatly reduce the calcination temperature, and save production costs.

[0074] The object of the present invention is to provide a staged roasting method for preparing high-purity manganese tetraoxide. The method uses a soluble manganese salt with high purity and low impurity content as a raw material, dissolves it in pure water and then spray-dries it to obtain a powder. The powder is then roasted at high temperature in a muffle furnace in an air or oxygen atmosphere to obtain a manganese tetraoxide precursor. The cooled and crushed precursor is then placed in a tube furnace and roasted at a lower temperature in a reducing gas atmosphere to obtain a crude manganese tetraoxide product. The crude product is pickled, crushed, washed, and dried. By roasting in two stages and setting different gas atmospheres, temperatures, and times, the particle size and purity of the product can be effectively regulated. The method has a simple production process, low cost, high safety, and is easy to implement industrially. The produced manganese tetraoxide has the characteristics of high product purity, low impurity content, uniform particle size distribution, high consistency, good activity, etc., and is suitable for the preparation of manganese-based positive electrode materials for lithium batteries.

[0075] The above examples are merely examples for clarification and are not intended to limit the embodiments. It should be noted that those skilled in the art may make several improvements and modifications without departing from the principles of the present invention, and such improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing high-purity manganese tetraoxide by a staged roasting method, It is characterized in that The specific steps include: Step 1: dissolve soluble manganese salt in pure water and stir to prepare a manganese salt solution; Step 2, preparing the manganese salt solution prepared in step 1 into manganese salt powder by a spray dryer; Step 3: Take an appropriate amount of the powder prepared in step 2 and place it in a muffle furnace for high-temperature calcination in air or oxygen atmosphere; Step 4: Cooling and crushing the trimanganese tetraoxide precursor prepared in step 3, placing it in a tube furnace, and calcining it in a reducing gas atmosphere; Step 5: pickling, crushing, washing and drying the manganese tetraoxide prepared in step 4.

2. The method for preparing high-purity manganese tetraoxide by a staged roasting method according to claim 1, Features: The soluble manganese salt used in step one is at least one of manganese chloride, acetate, sulfate or nitrate; the manganese concentration in the manganese solution prepared in step one is 40g / L-150g / L.

3. The method for preparing high-purity manganese tetraoxide by a staged roasting method according to claim 1, Features: The calcination temperature in step 3 is 200° C.-1000° C., and the calcination time in step 3 is 2 h-12 h.

4. The method for preparing high-purity manganese tetraoxide by a staged roasting method according to claim 3, Features: The calcination temperature in step 3 is 400° C.-600° C., and the calcination time in step 3 is 6 h-8 h.

5. The method for preparing high-purity manganese tetraoxide by a staged roasting method according to claim 1, Features: The calcination temperature used in step 4 is 100°C-700°C.

6. The method for preparing high-purity manganese tetraoxide by a staged roasting method according to claim 5, Features: The calcination temperature used in step 4 is 200°C-400°C.

7. The method for preparing high-purity manganese tetraoxide by a staged roasting method according to claim 1, Features: The calcination time in step 4 is 2h-6h.

8. The method for preparing high-purity manganese tetraoxide by a staged roasting method according to claim 1, Features: The reducing gas used in step 4 is one of hydrogen, carbon monoxide and methane.