Method for carrying out surface modification on high-nickel ternary positive electrode material by using mixed gas

By performing heat treatment under a mixed atmosphere on the surface of the high-nickel ternary positive electrode material, oxygen vacancy and CEI film are generated, the material mixing and discharging and side reaction problems are solved, the electrode performance and production costs are improved, and it is suitable for large-scale industrial applications.

CN118908299APending Publication Date: 2024-11-08XINXIANG TIANLI ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410879297.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-14
Filing Date
2024-07-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The mixed discharge phenomenon and material surface side reactions caused by the increase in nickel content in lithium-ion batteries affect the circulation performance and cost, and the effect of the existing technology modification methods is not outstanding.

Method used

Heat treatment is carried out under a mixed atmosphere to generate oxygen vacancies, increase layered structure stability, reduce residual alkali, and surface modification is carried out through different proportions of gas combination and process parameter control to form a CEI film to improve electrode performance.

Benefits of technology

The circulation performance and rate performance of high-nickel ternary cathode materials are improved, the production cost is reduced, and it is suitable for large-scale industrial production. The conductivity and reaction stability of the materials are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion battery electrode materials, and particularly relates to a method for carrying out surface modification on a high-nickel ternary positive electrode material by utilizing mixed gas. The method comprises the following steps: firstly, mixing a precursor and a lithium salt, then controlling process parameters such as gas flow and pressure intensity, and carrying out heat treatment at different stages through different types of mixed gases and different proportions, so as to obtain the surface-modified high-nickel ternary positive electrode material. The surface modification is mainly carried out on the surface of the high-nickel ternary material, so that the stability of a layered structure can be improved, and the surface of the material is coated with modified gas, so that relatively few crystal lattices release oxygen, the corrosion of electrolyte to the material is slowed down, and the electrochemical performance of the material is improved. The method for carrying out surface modification on the high-nickel ternary positive electrode material by using the mixed gas is low in cost, convenient to operate and convenient for large-scale production and application, and has a relatively good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery electrode materials, and specifically relates to a method for surface modification of high-nickel ternary positive electrode materials by using mixed gas. Background Art

[0002] Lithium-ion batteries are widely used in various portable electronic devices, electric vehicles and hybrid electric vehicles due to their high voltage, large capacity, no memory effect, long cycle life and environmental friendliness. Based on the wide range of uses of lithium-ion batteries, it is urgent to develop high-energy-density lithium-ion batteries with higher capacity, energy density, power density, longer cycle life and low cost.

[0003] High nickel ternary cathode materials (Ni≥0.6) have advantages over traditional lithium cobalt oxide, such as higher capacity, low toxicity and low cost. They are the mainstream cathode materials for high energy density lithium-ion power batteries and are widely studied and applied. However, as the nickel content increases, Ni 2+ and Li + Due to the close radius, mixing is more likely to occur, resulting in the attenuation of cycle performance and the reduction of specific capacity. In addition, residual alkali (LiOH, Li2CO3, etc.) is more likely to form on the surface of the material, which will not only cause surface side reactions, but also cause slurry agglomeration, affecting the coating effect.

[0004] In order to solve the above problems, domestic and foreign researchers have proposed strategies such as surface coating, lattice doping, core-shell and concentration gradient structure design, which effectively improved the electrochemical performance of the material. However, in actual application, due to factors such as production costs, the application effect of these implementation methods is not outstanding.

[0005] Therefore, the present invention conducts research work from the aspect of element doping surface modification, proposes to perform heat treatment in the atmosphere of mixed gas, perform certain modification on the material surface and generate oxygen vacancies, thereby promoting the formation of CEI film (cathode electrolyte interface film), increasing the stability of the layered structure, improving the stability of the electrode, and further improving the cycle performance and rate performance of the electrode. In addition, the use of mixed gas can reduce the residual alkali on the surface of the ternary material, and can further reduce the cost of high nickel ternary materials in large-scale industrial production. Summary of the invention

[0006] The purpose of the present invention is to provide a method for surface modification of high-nickel ternary positive electrode materials using mixed gas in view of the deficiencies in the prior art. The method firstly mixes the precursor and the lithium salt, then controls the process parameters such as the gas flow rate and pressure, and performs heat treatment at different stages by using different types of mixed gases and different proportions, thereby obtaining surface-modified high-nickel ternary positive electrode materials. The surface modification is mainly to increase the stability of the layered structure on the surface of the high-nickel ternary material, and to reduce the lattice oxygen release by coating the surface of the material with the modified gas, slowing down the corrosion of the material by the electrolyte, thereby improving the electrochemical performance of the material. The method of the present invention is a technology with low cost, easy operation, and suitable for large-scale industrial production.

[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0008] A method for surface modification of a high-nickel ternary positive electrode material using a mixed gas comprises the following steps:

[0009] (1) mixing a ternary material precursor and a lithium salt in a certain molar ratio to obtain a mixture base powder;

[0010] (2) placing the mixed substrate powder of step (1) in a tube furnace and introducing a surface modification gas;

[0011] (3) performing heat treatment under the ventilation conditions of step (2) to obtain a solid product;

[0012] (4) The solid product obtained in step (3) is crushed and sieved to finally obtain a surface-modified high-nickel ternary positive electrode material containing oxygen vacancies.

[0013] Preferably, the ternary material precursor in step (1) is Ni x Co y M z (OH)2, M is one or two of Mn and Al elements, wherein 0.6≤x≤0.9, 0.05≤y≤0.2, 0.05≤z≤0.2, x+y+z=1.

[0014] Further preferably, the ternary material precursor in step (1) is Ni 0.8 Co 0.1 Mn 0.1 (OH)2 (referred to as NCM811) or Ni 0.9 Co 0.05 Mn 0.05 (OH)2 (abbreviated as NCM90).

[0015] Preferably, the lithium salt in step (1) is one or more of lithium hydroxide, lithium carbonate and lithium nitrate.

[0016] Preferably, in step (1), the molar ratio of the ternary material precursor to the lithium salt is (0.8-1): (1-1.03).

[0017] Preferably, the modified gas introduced in step (2) is oxygen, nitrogen, ammonia, sulfur dioxide, hydrogen sulfide, or a combination of any two of these five gases, or a combination of any three of these five gases, or a combination of any four of these five gases, or a combination of all five gases.

[0018] Further preferably, in step (2), when the gas introduced is a single gas, specifically oxygen; when the gas introduced is a mixture of two gases, the ratio of the mixture is oxygen: other gas = (6-10): (1-4), and the other gas refers to nitrogen, ammonia, sulfur dioxide or hydrogen sulfide.

[0019] Further preferably, the ventilation method in step (2) can also be that after a period of time, the mixed gas of the two gases is introduced, pure oxygen is introduced instead.

[0020] Preferably, the gas introduction rate in step (2) is 0 to 1000 sccm, more preferably 40 sccm, 200 sccm, or 1000 sccm.

[0021] Preferably, the ventilation pressure in step (2) is 0-0.1 MPa, more preferably 0.01 MPa, 0.02 MPa, 0.05 MPa, 0.1 MPa.

[0022] Preferably, during the heat treatment process of step (3), the temperature stage of introducing the surface modification gas includes a heating stage, a heat preservation stage and / or a cooling stage. Specifically, the heat treatment conditions of step (3) are: firstly heating to 400-600°C at a rate of 3-5°C / min and keeping the temperature for 3-5h, then heating to 750-800°C at a rate of 3-5°C / min and keeping the temperature for 10-15h.

[0023] Specifically, the chemical formula of the surface-modified high-nickel ternary cathode material obtained in step (4) is: LiNi x Co y Mn z O2, where x+y+z=1, 0.6≤x≤0.9, 0.05≤y≤0.2, 0.05≤z≤0.2.

[0024] Further preferably, the chemical formula of the surface-modified high-nickel ternary positive electrode material obtained in step (4) is: LiNi 0.8 Co 0.1 Mn 0.1 O2 or LiNi 0.9 Co0.05 Mn 0.05 O2.

[0025] Furthermore, the surface-modified high-nickel ternary positive electrode material obtained by the surface modification method of the present invention has good capacitance and charge-discharge performance, and can be used to prepare lithium-ion batteries.

[0026] Furthermore, based on a general inventive concept, the present invention also provides the use of the surface-modified high-nickel ternary positive electrode material in the preparation of lithium-ion batteries.

[0027] Furthermore, the present invention also provides a method for preparing a lithium-ion battery using the surface-modified high-nickel ternary cathode material, which specifically comprises the following steps:

[0028] a. placing a certain amount of surface-modified high-nickel ternary cathode material, a conductive agent and a binder in a container to obtain a mixed powder;

[0029] b. Add a solvent to the mixed powder in step a, ultrasonically disperse it at a power of 80 to 100 W for 8 to 12 minutes, then place a polytetrafluoroethylene magnet in a container and stir it at a speed of 300 to 400 r / min for 8 to 12 hours to evenly disperse the high-nickel ternary cathode material and the conductive agent to obtain a mixed slurry;

[0030] c. The mixed slurry in step b is coated on aluminum foil (current collector), dried at 60-80°C for 8-12h, and then made into a button-type electrode sheet with a diameter of 12mm; then, in an argon-protected glove box, a metal lithium sheet is used as the negative electrode, a diaphragm is installed, and the electrolyte is a high-nickel 4.3V electrolyte. A button battery is assembled, and the battery model is a CR2032 button battery.

[0031] Specifically, in step a, the conductive agent is carbon black (Super-P); and the binder is PVDF.

[0032] Specifically, the solvent is selected from one of deionized water, ethanol and NMP.

[0033] Specifically, the mass of the solvent is 1 to 1.5 times the mass of the mixed powder.

[0034] Specifically, in the mixed slurry obtained in step b, the weight ratio of the surface-modified high-nickel ternary positive electrode material, the conductive agent, and the binder is (6-8):1:(1-2).

[0035] Specifically, the diaphragm type is a polypropylene diaphragm, and the main component of the electrolyte used in the battery is: lithium salt (lithium hexafluorophosphate); preferably, the electrolyte is 1M LiPF6 in EC:DEC=1:1vol%with 5% FEC.

[0036] Furthermore, based on a general inventive concept, the present invention also provides a lithium-ion battery prepared using the high-nickel ternary positive electrode material.

[0037] Compared with the prior art, the advantages of the present invention are:

[0038] 1. The present invention provides a method for surface modification of high-nickel ternary positive electrode materials using a mixed gas. Compared with the traditional sintering method, this method can modify the material surface in situ, which can achieve a certain coating effect, thereby stabilizing the layered structure of the material, reducing lattice oxygen release, and thus improving the conductivity and reaction stability of the material.

[0039] 2. The surface-modified high-nickel ternary positive electrode material prepared by the present invention can effectively reduce the residual alkali on the surface of the electrode material, and can also promote the formation of the CEI film, improve the stability of the electrode, and thus greatly improve the cycle performance of the battery.

[0040] 3. The method of using mixed gas to modify the surface of high-nickel ternary positive electrode materials described in the present invention is low-cost, easy to operate, convenient for large-scale production and application, and has good application prospects.

[0041] 4. The surface-modified high-nickel ternary positive electrode material obtained by the method of the present invention has a stable layered structure. The oxygen vacancies generated on the surface can reduce the release of lattice oxygen, reduce the generation of cracks inside the material, and reduce the surface residual alkali, thereby obtaining excellent electrochemical properties. The preparation method is safe and reliable, suitable for large-scale production, and can meet the development needs of the market. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 (a) XRD graph and (b) SEM graph of the high-nickel ternary positive electrode material prepared under the conditions of a ventilation rate of 1000 sccm and pure oxygen in Example 1;

[0043] Figure 2 (a) XRD and (b) SEM images of the high-nickel ternary positive electrode material NCM811-N prepared under the mixed gas condition of oxygen and nitrogen with a ratio of 8:2 in Example 2;

[0044] Figure 3 The EPR (oxygen vacancy) test of Example 1 and Example 2;

[0045] Figure 4 (a) XRD pattern and (b) SEM pattern of the high nickel ternary positive electrode material (NCM90) prepared in Example 3;

[0046] Figure 5(a) XRD pattern and (b) SEM pattern of the high nickel ternary cathode material NCM811-NH prepared under oxygen-ammonia mixed gas conditions in Example 5;

[0047] Figure 6 This is an XPS test graph of the high-nickel ternary positive electrode material prepared under the mixed gas condition of oxygen and nitrogen with a ratio of 8:2 in Example 2;

[0048] Figure 7 The SEM and EDS Mapping images of the high-nickel ternary positive electrode material prepared under the mixed gas condition of oxygen and nitrogen with a ratio of 8:2 in Example 2;

[0049] Figure 8 (a) Cycle performance and (b) rate performance diagram of high nickel ternary positive electrode materials prepared in Example 1 and Comparative Examples 1 and 2;

[0050] Fig. 9 The (a) cycle performance and (b) rate performance diagrams of high nickel ternary positive electrode materials modified by mixed gases of different proportions in Examples 1 and 2 and Comparative Examples 3, 4 and 5. DETAILED DESCRIPTION

[0051] The following examples will further illustrate the present invention in conjunction with the accompanying drawings. This embodiment is implemented based on the technical solution of the present invention, and provides detailed implementation methods and processes, but the protection scope of the present invention is not limited to the following embodiments.

[0052] The experimental methods in the following examples without specifying specific conditions are generally carried out under conventional conditions, and the raw materials and reagents used are conventional commercially available products unless otherwise specified.

[0053] The ternary material precursors NCM811 and NCM90 involved in the comparative examples and embodiments are both provided by Henan Xinxiang Tianli Lithium Energy Co., Ltd., and their preparation methods can adopt conventional methods in the prior art, which are not the inventive point of the present invention, so they will not be described in detail.

[0054] Example 1

[0055] Example 1 provides a method for surface modification of a high-nickel ternary positive electrode material, the specific steps of which are:

[0056] 1) Using nickel sulfate, cobalt sulfate and manganese sulfate as raw materials, the ternary material precursor Ni was prepared by coprecipitation method. 0.8 Co 0.1 Mn 0.1 (OH)2 (referred to as NCM811), the ternary material precursor Ni 0.8 Co 0.1 Mn 0.1The specific preparation method of (OH)2 can be prepared by conventional methods in the prior art, and is not the inventive point of the present invention, so it will not be described in detail;

[0057] The ternary material precursor NCM811 (powder) and lithium hydroxide monohydrate are mixed at a molar ratio of 1:1.03 to obtain a mixture base powder;

[0058] 2) The mixed substrate powder of step 1) is loaded into a porcelain boat, and then placed in a tube furnace, and oxygen is continuously introduced at a ventilation rate of 1000 sccm and a pressure of 0.05 MPa;

[0059] 3) performing heat treatment while introducing oxygen in step 2), wherein the specific process is: firstly heating to 500° C. at a rate of 5° C. / min and keeping the temperature for 4 hours, then heating to 780° C. at a rate of 5° C. / min and keeping the temperature for 12 hours, then stopping heating and allowing the temperature to cool naturally, and maintaining the introduction of oxygen during the whole process to obtain a solid product;

[0060] 4) The solid product obtained in step 3) is crushed and sieved to finally obtain the surface-modified NCM811 high-nickel ternary positive electrode material (LiNi 0.8 Co 0.1 Mn 0.1 O2).

[0061] The XRD spectrum of the surface modified high nickel ternary cathode material prepared in this example is as follows: Figure 1 As shown in a, observe Figure 1 a It can be seen that the XRD diffraction peak belongs to the α-NaFeO2 layered structure and the R-3m space group; there is no other impurity phase, indicating that a relatively pure high-nickel ternary positive electrode material is obtained.

[0062] The SEM image of the surface modified high nickel ternary cathode material prepared in this example is as follows: Figure 1 As shown in b, observe Figure 1 b It can be seen that the particle size of the prepared material is ~10μm, the morphology is regular, and there are no cracks on the surface, indicating that the prepared surface-modified high-nickel ternary positive electrode material has a good structure.

[0063] Example 2

[0064] Example 2 provides a method for surface modification of a high-nickel ternary positive electrode material. The difference between Example 2 and Example 1 is that the gas introduced in step 2) is a mixture of oxygen and nitrogen, and the volume ratio of the mixture is oxygen: nitrogen = 8:2, and finally a surface-modified NCM811-N high-nickel ternary positive electrode material is obtained.

[0065] The XRD spectrum of the surface modified high nickel ternary cathode material prepared in this example is as follows: Figure 2 As shown in a, observe Figure 2 It can be seen from a that the attribution of the XRD diffraction peak is no different from that in Example 1, indicating that a relatively pure high-nickel ternary positive electrode material is obtained.

[0066] The SEM image of the surface modified high nickel ternary cathode material prepared in this example is as follows: Figure 2 As shown in b, observe Figure 2 b It can be seen that the obtained high-nickel ternary positive electrode material has a regular morphology and uniform particle size, and there is no obvious difference from that in Example 1.

[0067] The EPR oxygen vacancy tests were carried out on Example 2 and Example 1, and the results are as follows: Figure 3 As shown, from Figure 3 It can be seen that the addition of the mixed gas of Example 2 increases the oxygen vacancies on the surface of the high-nickel ternary positive electrode material, indicating that the mixed gas successfully modified the surface of the high-nickel ternary positive electrode material and increased the oxygen vacancies in the material.

[0068] Example 3

[0069] Example 3 provides a method for surface modification of a high-nickel ternary positive electrode material. The difference between Example 3 and Example 1 is that the ternary material precursor used in step 1) is Ni 0.9 Co 0.05 Mn 0.05 (OH)2 (abbreviated as NCM90, the NCM90 is prepared by coprecipitating nickel sulfate, cobalt sulfate and manganese sulfate in a molar ratio of 9:0.5:0.5 with ammonia water and then heat treating the mixture. The specific preparation method can be a conventional method in the prior art, and it is not the inventive point of the present invention, so it will not be repeated here), and finally the surface-modified NCM90 high-nickel ternary positive electrode material (LiNi 0.9 Co 0.05 Mn 0.05 O2).

[0070] The XRD spectrum of the surface modified NCM90 high nickel ternary cathode material prepared in this example is as follows: Figure 4 As shown in a, observe Figure 4 It can be seen from a that the attribution of the XRD diffraction peak is no different from that in Example 1, indicating that a relatively pure high-nickel ternary positive electrode material is obtained.

[0071] The SEM image of the surface modified high nickel ternary cathode material prepared in this example is as follows: Figure 4 As shown in b, observe Figure 4 b It can be seen that the particle size of the prepared material is ~10μm, the morphology is regular, and there are no cracks on the surface, indicating that the prepared high-nickel ternary positive electrode material has a good structure.

[0072] Example 4

[0073] Example 4 provides a method for surface modification of a high-nickel ternary positive electrode material. The difference between Example 4 and Example 1 is that in step 3), a mixed gas with a volume ratio of oxygen: nitrogen = 8:2 is first introduced until the temperature is raised to 500°C and kept warm for 4 hours, and then the gas is replaced with pure oxygen, and then the temperature is raised to 780°C and kept warm for 12 hours, and the heating rate is 5°C / min.

[0074] Example 5

[0075] Example 5 provides a method for surface modification of a high-nickel ternary positive electrode material. The difference between Example 5 and Example 1 is that the gas introduced in step 2) is a mixture of oxygen and ammonia, and the volume ratio of the mixture is oxygen: ammonia = 8:2, and finally a surface-modified NCM811-NH high-nickel ternary positive electrode material is obtained.

[0076] The XRD spectrum of the surface modified NCM811-NH high nickel ternary cathode material prepared in this example is shown in Figure 5 As shown in a, observe Figure 5 It can be seen from a that the XRD diffraction peak is attributed to the α-NaFeO2 layered structure and the R-3m space group, which is no different from that in Example 1, indicating that a relatively pure high-nickel ternary positive electrode material is obtained.

[0077] The SEM image of the surface modified high nickel ternary cathode material prepared in this example is as follows: Figure 5 As shown in b, the particle size of the prepared material is ~10μm, the morphology is regular, and there are no cracks on the surface, indicating that the prepared surface-modified high-nickel ternary positive electrode material has a good structure.

[0078] Performance Testing

[0079] The high nickel ternary positive electrode material prepared in Example 2 was tested by XPS and SEM EDS Mapping. The results are as follows Figure 6 and Figure 7 As shown in the XPS graph, when the oxygen-nitrogen ratio is 8:2, the high-nickel ternary positive electrode material obtained has nitrogen doped on its surface, and a portion of Li3N is generated therein, and Li3N has the function of promoting the formation of CEI film, improving the stability of the electrode material, and further improving the high cycle performance and rate performance of the electrode, which is consistent with the expected effect of the present invention.

[0080] In addition, the presence of nitrogen on the surface of the material can also be observed through SEM EDS Mapping. Therefore, it can also be explained that when the oxygen-nitrogen ratio is 8:2, Li3N is generated on the surface of the high-nickel ternary positive electrode material.

[0081] Comparative Example 1

[0082] Comparative Example 1 provides a method for surface modification of a high-nickel ternary positive electrode material, the specific steps of which are:

[0083] 1) Using nickel sulfate, cobalt sulfate and manganese sulfate as raw materials, the ternary material precursor Ni was prepared by coprecipitation method. 0.8 Co 0.1 Mn 0.1 (OH)2 (referred to as NCM811), the ternary material precursor Ni 0.8 Co 0.1 Mn 0.1 The specific preparation method of (OH)2 can be prepared by conventional methods in the prior art, and is not the inventive point of the present invention, so it will not be described in detail;

[0084] The ternary material precursor NCM811 (powder) and lithium hydroxide monohydrate are mixed at a molar ratio of 1:1.03 to obtain a mixture base powder;

[0085] 2) The mixed substrate powder of step 1) is loaded into a porcelain boat, and then placed in a tube furnace, and a mixed gas of oxygen and nitrogen is continuously introduced at a ventilation rate of 200 sccm and a pressure of 0.05 MPa, wherein the volume ratio of the mixed gas is oxygen: nitrogen = 8:2;

[0086] 3) performing heat treatment while introducing the mixed gas in step 2), wherein the temperature is first raised to 500° C. at a rate of 5° C. / min and kept at this temperature for 4 hours, then raised to 780° C. at a rate of 5° C. / min and kept at this temperature for 12 hours, then the heating is stopped and the temperature is naturally lowered, and oxygen is introduced during the whole process to obtain a solid product;

[0087] 4) The solid product obtained in step 3) is crushed and sieved to finally obtain a surface-modified high-nickel ternary positive electrode material.

[0088] Comparative Example 2

[0089] Comparative Example 2 provides a method for surface modification of a high-nickel ternary positive electrode material. The difference between Comparative Example 2 and Comparative Example 1 is that the ventilation rate in step 2) is 40 sccm.

[0090] Comparative Example 3

[0091] Comparative Example 3 provides a method for surface modification of a high-nickel ternary positive electrode material. The difference between Comparative Example 3 and Comparative Example 1 is that the ventilation rate in step 2) is 1000 sccm, and the mixing ratio of oxygen and nitrogen in the mixed gas is 9:1.

[0092] Comparative Example 4

[0093] Comparative Example 4 provides a method for surface modification of a high-nickel ternary positive electrode material. The difference between Comparative Example 4 and Comparative Example 1 is that the ventilation rate in step 2) is 1000 sccm, and the mixing ratio of oxygen and nitrogen in the mixed gas is 7:3.

[0094] Comparative Example 5

[0095] Comparative Example 5 provides a method for surface modification of a high-nickel ternary positive electrode material. The difference between Comparative Example 5 and Comparative Example 1 is that the ventilation rate in step 2) is 1000 sccm, and the mixing ratio of oxygen and nitrogen in the mixed gas is 6:4.

[0096] Application test 1

[0097] The LiNi prepared in Example 1 0.8 Co 0.1 Mn 0.1 O2 (abbreviated as NCM811) high nickel ternary positive electrode material is used for lithium-ion batteries. The specific preparation method is as follows:

[0098] a. The NCM811 high-nickel ternary cathode material prepared in Example 1 was mixed with carbon black (Super-P, conductive agent, Shenzhen Kejing Zhida Technology Co., Ltd., CAS1333-86-4) and a binder PVDF according to a mass ratio of 8:1:1 (specifically 400 mg, 50 mg, and 50 mg, respectively) to obtain a mixed powder;

[0099] b. Then add the mixed powder in step a to the solvent (N-methylpyrrolidone, NMP) and place it in a mixing container to mix evenly. The mass of the solvent is 1.5 times the mass of the mixed powder. Then, ultrasonically disperse it at a power of 100 W for 8 minutes. Then, place a polytetrafluoroethylene magnet in the mixing container and stir it at a speed of 400 r / min for 10 hours to evenly disperse the NCM811 high-nickel ternary positive electrode material and carbon black (Super-P) to obtain a mixed slurry.

[0100] c. The mixed slurry in step b is coated on aluminum foil and dried at 80°C for 10 hours to prepare an electrode; then, in an argon-protected glove box, a metal lithium sheet is used as the negative electrode, the electrolyte is a high-nickel 4.3V electrolyte (1M LiPF6, DEC:EC=1:1Vol% with 5%FEC), and a polypropylene diaphragm is used to assemble a button battery, and the battery model is a CR2032 button battery.

[0101] Then the electrochemical performance test was carried out. The test conditions for the cycle performance were as follows: the charge and discharge cut-off voltage was 3.0-4.3V, and the test current was 1.0C (1C = 180mAg -1); the test conditions for rate performance are as follows: the charge and discharge cut-off voltage is 3.0-4.3V, and the test current is 0.1C, 0.2C, 0.5C, 1.0C, 3.0C, 0.1C.

[0102] Similarly, the ternary cathode materials prepared in Comparative Examples 1 and 2 were assembled into lithium-ion button cells using the above method, and the electrochemical performance was tested under the same test conditions. Figure 8 As shown in a, the rate performance diagram is shown in 8b.

[0103] from Figure 8 It can be seen from a that the ternary cathode material prepared in Example 1 at a ventilation rate of 1000 sccm exhibits excellent electrochemical performance, with an initial capacity of up to 187 mAh / g, much higher than 165 mAh / g at 200 sccm and 138 mAh / g at 40 sccm; similarly, Figure 8 In the test of b, the ternary cathode material prepared in Example 1 at a ventilation rate of 1000 sccm also showed excellent rate performance, showing 218, 210, 201, 185, 170, and 213 mAh g at current densities of 0.1C, 0.2C, 0.5C, 1C, 3C, and 0.1C. -1 The specific capacity is much higher than 198, 190, 180, 175, 158, 200 mAh g at 200 sccm. -1 and 155, 145, 139, 125, 114, 156 mAh g at 40 sccm -1 , showing excellent electrochemical performance.

[0104] Application Test 2

[0105] The lithium-ion battery was prepared in the same manner as in application test 1, and the electrochemical performance test was carried out in the same manner and under the same test conditions.

[0106] Application test 2 mainly assembles button batteries with the ternary materials of Examples 1 and 2 and Comparative Examples 3, 4, and 5 and tests the electrochemical performance. Cycle performance Fig. 9 As shown in a, the rate performance diagram is shown in 9b.

[0107] from Fig. 9It can be clearly seen from the cycle performance of a that although the specific capacity of the high nickel ternary positive electrode material prepared under pure oxygen conditions in Example 1 is higher at the beginning of the cycle, its capacity decays rapidly as the cycle proceeds, while the cycle performance of the high nickel ternary positive electrode material prepared using the mixed gas in Example 2 and Comparative Examples 3, 4, and 5 is relatively stable, and the high nickel ternary positive electrode material prepared when the oxygen-nitrogen ratio is 8:2 has an initial specific capacity of 183 mAh / g and 184 mAh / g after 200 cycles, and the capacity has not decreased but has slightly increased.

[0108] Fig. 9 In b, in the rate performance test, the specific capacity of the high nickel ternary cathode material prepared under the condition of 8:2 in Example 2 at 0.1C is 202mAh / g. After a series of current densities, the capacity is restored to 204mAh / g when it returns to 0.1C, and its capacity recovery rate is as high as 101%, which is much higher than that of high nickel ternary materials under other atmosphere treatments. In contrast, the high nickel ternary cathode material prepared under the condition of oxygen-nitrogen ratio of 8:2 in Example 2 exhibits the best electrochemical performance.

[0109] The method of using mixed gas to modify the surface of high-nickel ternary positive electrode materials described in the present invention not only simplifies the modification method of ternary positive electrode materials in the prior art but also improves its overall performance, has good application value, and is suitable for process promotion and application.

[0110] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for surface modification of high-nickel ternary positive electrode materials using a mixed gas, characterized in that: The following steps are involved: (1) mixing the ternary material precursor and the lithium salt in a certain molar ratio to obtain a mixture base powder; (2) placing the mixed base powder of step (1) in a container and introducing a surface modification gas; (3) performing heat treatment under the ventilation conditions of step (2) to obtain a solid product; (4) The solid product obtained in step (3) is crushed and sieved to finally obtain a surface-modified high-nickel ternary positive electrode material containing oxygen vacancies.

2. The method according to claim 1, characterized in that The ternary material precursor in step (1) is Ni x Co y M z (OH)2, M is one or two of Mn and Al elements, wherein 0.6≤x≤0.9, 0.05≤y≤0.2, 0.05≤z≤0.2, x+y+z=1.

3. The method according to claim 1, characterized in that The lithium salt in step (1) is one or more of lithium hydroxide, lithium carbonate and lithium nitrate; the molar ratio of the ternary material precursor to the lithium salt in step (1) is (0.8~1):(1~1.03).

4. The method according to claim 1, characterized in that The modified gas introduced in step (2) is oxygen, nitrogen, ammonia, sulfur dioxide, hydrogen sulfide, or a combination of any two of these five gases, or a combination of any three of these five gases, or a combination of any four of these five gases, or a combination of all five gases.

5. The method according to claim 1, characterized in that In step (2), when the gas introduced is a single gas, specifically oxygen; when the gas introduced is a mixture of two gases, the ratio of the mixture is oxygen: other gas = (6-10): (1-4), and the other gas refers to nitrogen, ammonia, sulfur dioxide or hydrogen sulfide.

6. The method according to claim 1, characterized in that The gas introduction rate in step (2) is 0~1000sccm; the ventilation pressure in step (2) is 0~0.1 MPa.

7. The method according to claim 1, characterized in that The heat treatment conditions in step (3) are: first, heating to 400-600°C at a rate of 3-5°C / min and keeping the temperature for 3-5 h, then heating to 750-800°C at a rate of 3-5°C / min and keeping the temperature for 10-15 h.

8. The method according to claim 1, characterized in that The chemical formula of the surface-modified high-nickel ternary cathode material obtained in step (4) is: LiNi x Co y Mn z O2, where x+y+z=1, 0.6≤x≤0.9, 0.05≤y≤0.2, 0.05≤z≤0.

2.

9. A surface-modified high-nickel ternary positive electrode material prepared by the method according to any one of claims 1 to 8.

10. Use of the surface-modified high-nickel ternary positive electrode material according to claim 9 in the preparation of lithium-ion batteries.