Lithium manganese iron phosphate modified high-voltage lithium nickel manganese oxide positive electrode material and preparation method thereof
Through the nano-coated coating of lithium manganese iron phosphate and high-temperature and high-pressure reaction technology, the problems of high-pressure nickel lithium manganese oxide materials in the hydrothermal coating process are solved, and the conductive and cyclic stability of the materials are improved. Suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202410972223.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing high-pressure lithium nickel manganate LiNi0.5Mn1.5O4 material has settlement problems during hydrothermal coating, resulting in uneven coating and complex preparation processes, affecting the cyclic performance of the material.
The method of uniformly coating lithium nickel manganese manganese oxide by nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- nano- Oxythiophene): Polystyrene sulfonate (PEDOT:PSS) is used as an additive to simplify the process flow and improve the coating effect.
The conductivity and stability of the material are improved, the material distortion during lithium ions is reduced, and the dissolution of manganese and nickel transition metals is inhibited, which significantly improves the cycle stability of the battery and the adaptability of industrial production.
Smart Images

Figure CN118908302A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of lithium ion battery positive electrode materials, in particular to lithium manganese iron phosphate modified high-voltage lithium nickel manganese oxide positive electrode materials and a preparation method thereof. Background Art
[0002] With the continuous development of electronic equipment such as spacecraft, electric vehicles, medical equipment and communication equipment, lithium-ion batteries have become an indispensable part of them; however, their energy density needs to be further improved to meet the application in new energy vehicles.
[0003] The energy density of a single lithium-ion battery is determined by the operating voltage and capacity of the battery itself. Therefore, the energy density of the battery can be increased by increasing the operating voltage or capacity of the battery. 0.5 Mn 1.5 O4 material (LNMO) has a high working voltage (4.7V) and capacity (148mA / g), and is considered to be an ideal high energy density lithium ion battery cathode material. 0.5 Mn 1.5 There is a certain amount of Mn in O4 material 3+ , Mn 3+ Disproportionation reaction may occur, resulting in a reduction in active substances and unstable results, leading to reduced material cycle performance. To solve this problem, LNMO is usually modified by ion doping and surface coating.
[0004] As an upgraded product of lithium iron phosphate, lithium iron manganese phosphate can be used as a modified material for LNMO due to its high voltage platform (4.1V) and cyclic structural stability. Chinese invention patent publication number CN112885995A discloses a method for manufacturing a lithium iron manganese phosphate-coated high-voltage lithium nickel manganese oxide positive electrode material. The invention is to disperse the LNMO material in a lithium iron manganese phosphate precursor solution, and to coat the lithium iron manganese phosphate on the surface of the lithium nickel manganese oxide by a hydrothermal method for modification. However, this method has defects: that is, when the LNMO material is hydrothermally coated in the solution, since the solution is in a static state, the LNMO material is easy to settle, resulting in uneven coating and deviation between the coating amount and the theoretical amount, and the preparation process of this method is complicated and the operation is relatively difficult. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material, so that the lithium iron manganese phosphate is nano-sized and evenly coated with lithium nickel manganese oxide, thereby improving the electrochemical performance; the present invention also provides a simple and efficient preparation method.
[0006] The method for preparing the lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material of the present invention comprises the following steps:
[0007] (1) uniformly mixing the manganese source, nickel source, lithium source and additive in a ball mill, and adding water or ethanol to assist dispersion;
[0008] (2) The dispersed mixture is dried and ground into powder, sintered and annealed to obtain LiNi 0.5 Mn 1.5 O4 material;
[0009] (3) According to the chemical formula of lithium manganese iron phosphate, LiMn x Fe (1-x) PO4, x is 0.5-0.7, dissolve the manganese source, iron source, phosphorus source, carbon source, lithium source and additives in water, and then add LiNi 0.5 Mn 1.5 O4 material is stirred evenly to obtain a composite slurry, wherein the second additive is poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (ie, PEDOT:PSS).
[0010] (4) introducing nitrogen into a high-temperature and high-pressure reactor containing the composite slurry, heating and pressurizing the slurry under stirring to change the slurry into a supercritical state, and cooling and releasing the pressure after the reaction in this state to obtain a post-reaction slurry;
[0011] (5) After the reaction, the slurry is filtered and dried to obtain the product.
[0012] Preferably, in step (1), the mixing time is 1 to 12 hours, preferably 4 hours; and the solid content after adding water or ethanol is 20%.
[0013] Preferably, in step (1), the manganese source is at least one of manganese dioxide, manganese carbonate, and manganese tetroxide, the nickel source is nickel acetate, the lithium source is lithium carbonate, and the additive one is at least one of magnesium carbonate, aluminum hydroxide, chromium oxide, titanium oxide, niobium oxide, and aluminum fluoride, and the amount of additive one added is 1% to 5% of the total mass of the nickel source and the manganese source.
[0014] Preferably, in step (2), the drying temperature is 120° C. and the drying time is 12 h.
[0015] Preferably, in step (3), the manganese source is at least one of manganese sulfate, manganese nitrate, and manganese acetate; the iron source is at least one of iron nitrate and iron sulfate; the lithium source is at least one of lithium carbonate and lithium hydroxide; the phosphorus source is at least one of phosphoric acid and diammonium phosphate; and the carbon source is at least one of glucose and sucrose.
[0016] Preferably, in step (2), the temperature is raised from room temperature to 800°C to 900°C at a rate of 4 to 6°C / min, sintered for 8h to 16h, and then annealed to 600°C to 700°C and kept warm for 4h to 8h; more preferably, the temperature is raised to 850°C at a rate of 5°C / min, sintered for 12h, and annealed to 700°C and kept warm for 6h.
[0017] Preferably, in step (3), LiMn x Fe (1-x) The mass of PO4 accounts for the mass of LiNi 0.5 Mn 1.5 O4 material and LiMn x Fe (1-x) 5% to 20% of the total mass of PO4.
[0018] Preferably, in step (3), the molar amount of the additive 2 is 1% to 5% of the total molar amount of Mn and Fe in the manganese source and the iron source.
[0019] Preferably, in step (4), the temperature of the reactor is 350-400°C, the pressure is 25-30 MPa, and the time is 20-30 min.
[0020] The lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material of the present invention is prepared by the above-mentioned preparation method.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention uses poly (3,4-ethylenedioxythiophene): polystyrene sulfonate (PEDOT:PSS) as an additive, which has the characteristics of high conductivity, chemical stability, thermal stability, etc., and is coated on the surface of the material to reduce the interface resistance between the positive electrode and the electrolyte, thereby improving the conductivity and stability of the material;
[0023] 2. The present invention uses a supercritical method to convert nano-LiMn into x Fe (1-x) PO4 is evenly coated on LiNi 0.5 Mn 1.5 O4 surface, compared with the traditional mechanical ball milling and hydrothermal coating, it is more fine and uniform; and this method is to coat LiMn x Fe (1-x) PO4 is coated on LiNi in one step 0.5 Mn 1.5 O4 surface, reducing the conventional preparation of LiMn x Fe (1-x) The high-temperature sintering and other process steps required by PO4 have a simple process flow and a fast reaction rate, making it suitable for large-scale industrial production;
[0024] 3. As for material performance, the present invention improves structural stability, which can not only reduce the distortion of the material during lithium ion insertion and extraction, but also inhibit the dissolution of manganese and nickel transition metals from the material, thereby effectively improving the cycle stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a SEM image of the material obtained in Example 1;
[0026] Figure 2 is the XRD pattern of the material obtained in Example 1;
[0027] Figure 3 It is a cycle comparison diagram of Examples 1, 2 and Comparative Example 1. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and embodiments.
[0029] Unless otherwise specified, all raw materials used in the examples are commercially available.
[0030] Example 1
[0031] (1) Electrolytic manganese tetraoxide and nickel acetate were weighed at a molar ratio of Mn:Ni of 3:1, lithium carbonate was weighed at a molar number of Li:total molar number of Mn and Ni of 1.06:2, magnesium carbonate was weighed at 5% of the total mass of manganese tetraoxide and nickel acetate, ethanol was used as a dispersant, and the solid content during dispersion was 20%, and the mixture was placed in a ball mill and mixed for 4 hours at 25°C;
[0032] (2) The mixture was dried at 120°C for 12 hours, transferred to a muffle furnace, heated to 850°C at a rate of 5°C / min, and sintered for 12 hours; annealed to 700°C, kept at a constant temperature for 6 hours, and cooled to obtain LiNi 0.5 Mn 1.5 O4 material;
[0033] (3) Manganese sulfate and ferric sulfate were weighed at a molar ratio of Mn:Fe of 6:4 to prepare a solution with a total molar concentration of 0.1 mol / L of manganese sulfate and ferric sulfate. The molar number of Li: the total molar number of Mn and Fe was 1.02:1. Lithium hydroxide was weighed at a molar number of P: the total molar number of Mn and Fe was 1:1. Ammonium dihydrogen phosphate was weighed at a molar number of P: the total molar number of Mn and Fe was 1:1. The theoretically prepared LiMn 0.6 Fe 0.4 Glucose was weighed at 5% of the mass of PO4, and PEDOT:PSS was weighed at 2% of the total molar number of Mn and Fe. The above raw materials were added into a high-temperature and high-pressure reactor and stirred evenly; the theoretically prepared LiMn 0.6 Fe 0.4 Weigh the mass of PO4 to obtain LiNi 0.5Mn 1.5 O4 material (LiMn 0.6 Fe 0.4 PO4 accounts for LiNi 0.5 Mn 1.5 O4 materials and LiMn 0.6 Fe 0.4 5% of the total mass of PO4) was added into the reactor and stirred evenly;
[0034] (4) The high temperature and high pressure reactor was continuously stirred, nitrogen was introduced, the temperature was controlled at 400°C, the pressure was 25 MPa, the reaction was carried out for 20 min, the slurry was filtered and dried after depressurization and cooling, and a nano-scale lithium manganese iron phosphate modified high pressure lithium nickel manganese oxide positive electrode material (coating amount 5%) was obtained, which was recorded as C / LiMn 0.6 Fe 0.4 PO4(5%)@LiNi 0.5 Mn 1.5 O4 material.
[0035] Example 2
[0036] The difference between Example 2 and Example 1 is that in step (2), the theoretically prepared LiMn 0.6 Fe 0.4 PO4 accounts for the amount of LiNi 0.5 Mn 1.5 O4 materials and LiMn 0.6 Fe 0.4 10% of the total mass of PO4.
[0037] Example 3
[0038] The difference between Example 3 and Example 1 is that in step (2), the theoretically prepared LiMn 0.6 Fe 0.4 PO4 accounts for the amount of LiNi 0.5 Mn 1.5 O4 materials and LiMn 0.6 Fe 0.4 15% of the total mass of PO4.
[0039] Example 4
[0040] The difference between Example 4 and Example 1 is that in step (2), the theoretically prepared LiMn 0.6 Fe 0.4 PO4 accounts for the amount of LiNi 0.5 Mn 1.5 O4 materials and LiMn 0.6 Fe 0.4 20% of the total mass of PO4.
[0041] Comparative Example 1
[0042] This comparative example 1 uses the LiNi obtained according to step (1) in Example 1 0.5 Mn 1.5 O4 material.
[0043] Comparative Example 2
[0044] (1) Manganese sulfate and ferric sulfate were weighed at a molar ratio of Mn:Fe of 6:4 to prepare a solution with a total molar concentration of 0.1 mol / L of manganese sulfate and ferric sulfate. The molar number of Li: the total molar number of Mn and Fe was 1.02:1. Lithium hydroxide was weighed at a molar number of P: the total molar number of Mn and Fe was 1:1. Ammonium dihydrogen phosphate was weighed at a molar number of P: the total molar number of Mn and Fe was 1:1. The theoretically prepared LiMn 0.6 Fe 0.4 Weigh glucose at 5% of the mass of PO4 and weigh PEDOT:PSS at 2% of the total molar number of Mn and Fe, add the above raw materials into a high-temperature and high-pressure reactor and stir evenly;
[0045] (2) The high temperature and high pressure reactor is continuously stirred, nitrogen is introduced, the temperature is controlled at 400°C, the pressure is 25 MPa, the reaction is carried out for 20 minutes, the pressure is released and the slurry is filtered and dried after cooling to obtain nano-sized lithium iron manganese phosphate LiMn 0.6 Fe 0.4 PO4 material;
[0046] (3) LiNi prepared in Comparative Example 1 0.5 Mn 1.5 O4 material and LiMn 0.6 Fe 0.4 PO4 material (according to LiMn 0.6 Fe 0.4 PO4 material accounts for LiNi 0.5 Mn 1.5 O4 materials and LiMn 0.6 Fe 0.4 5% of the total mass of PO4) was weighed and mechanically mixed in a ball mill to obtain a mixed material as a positive electrode material.
[0047] Comparative Example 3
[0048] (1) Electrolytic manganese tetraoxide and nickel acetate were weighed at a molar ratio of Mn:Ni of 3:1, lithium carbonate was weighed at a molar number of Li: the total molar number of Mn and Ni of 1.06:2, magnesium carbonate was weighed at 5% of the total mass of manganese tetraoxide and nickel acetate, and ethanol was weighed as a dispersant at a solid content of 20%, and the mixture was placed in a ball mill and mixed for 4 hours at 25°C;
[0049] (2) The mixture was dried at 120°C for 12 hours, transferred to a muffle furnace, heated to 850°C at a rate of 5°C / min, and sintered for 12 hours; annealed to 700°C, kept at a constant temperature for 6 hours, and cooled to obtain LiNi 0.5 Mn 1.5 O4 material;
[0050] (3) Manganese sulfate and ferric sulfate were weighed at a molar ratio of Mn:Fe of 6:4 to prepare a solution with a total molar concentration of 0.1 mol / L of manganese sulfate and ferric sulfate. The molar number of Li: the total molar number of Mn and Fe was 1.02:1. Lithium hydroxide was weighed at a molar number of P: the total molar number of Mn and Fe was 1:1. Ammonium dihydrogen phosphate was weighed at a molar number of P: the total molar number of Mn and Fe was 1:1. The theoretically prepared LiMn 0.6 Fe 0.4 PO4 mass 5% of glucose was weighed, the above raw materials were added into a high temperature and high pressure reactor and stirred evenly; the theoretically prepared LiMn 0.6 Fe 0.4 Weigh the mass of PO4 to obtain LiNi 0.5 Mn 1.5 O4 material (LiMn 0.6 Fe 0.4 PO4 accounts for LiNi 0.5 Mn 1.5 O4 materials and LiMn 0.6 Fe 0.4 5% of the total mass of PO4) was added into the reactor and stirred evenly;
[0051] (4) The high temperature and high pressure reactor was continuously stirred, nitrogen was introduced, the temperature was controlled at 400°C, the pressure was 25 MPa, the reaction was carried out for 20 min, the slurry was filtered and dried after depressurization and cooling, and a nano-scale lithium manganese iron phosphate modified high pressure lithium nickel manganese oxide positive electrode material (coating amount 5%) was obtained, which was recorded as C / LiMn 0.6 Fe 0.4 PO4(5%)@LiNi 0.5 Mn 1.5 O4 material.
[0052] Performance Testing
[0053] The discharge capacity and capacity retention rate of Examples 1-4 and Comparative Examples 1-3 were tested, and the results are shown in Table 1.
[0054] Table 1 Discharge capacity and capacity retention rate test of Examples 1-4 and Comparative Examples 1-3
[0055] sample 0.2C discharge capacity mAh / g Capacity retention rate (200 cycles) Example 1 135.8 83.75% Example 2 134.6 85.69% Example 3 133.4 86.54% Example 4 132.3 87.35% Comparative Example 1 136.2 80.67% Comparative Example 2 135.4 81.98% Comparative Example 3 135.6 82.45%
[0056] from Figure 1 It can be seen that the present invention forms lithium manganese iron phosphate coated with lithium nickel manganese oxide on the surface. Figure 2The XRD diagram of the positive electrode material obtained in Example 1 shows characteristic diffraction peaks of lithium iron manganese phosphate and lithium nickel manganese oxide, indicating that the target material has been synthesized; Figure 3 For the comparison of the cycle trends of Comparative Example 1 and Examples 1 and 2, Figure 3 It can be seen that the cycle retention rate of lithium iron manganese phosphate coated lithium nickel manganese oxide material is better than that of the uncoated material, and the higher the coating amount, the better the cycle retention rate; combined with Table 1, from Examples 1-4 and Comparative Example 1, as the coating amount of lithium iron manganese phosphate increases, the discharge capacity decreases, but the cycle retention rate increases significantly; from Example 1 and Comparative Example 2, the cycle performance of lithium iron manganese phosphate coated on the surface of lithium nickel manganese oxide by supercritical method is better than that of simple mechanical mixing, indicating that the coating method is more uniform; from Example 1 and Comparative Example 3, the use of the additive poly (3,4-ethylenedioxythiophene): polystyrene sulfonate (PEDOT:PSS) helps to improve the cycle performance of the coated material; it shows that the present invention has a good effect on LiNi 0.5 Mn 1.5 The recycling performance of O4 materials has been significantly improved.
Claims
1. A method for preparing a lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material, characterized in that: The following steps are involved: (1) uniformly mixing a manganese source, a nickel source, a lithium source and an additive in a ball mill; (2) The dispersed mixture is dried and ground into powder, sintered and annealed to obtain LiNi 0.5 Mn 1.5 O4 material; (3) According to the chemical formula of lithium manganese iron phosphate, LiMn x Fe (1-x) PO4, x is 0.5-0.7, dissolve the manganese source, iron source, phosphorus source, carbon source, lithium source and additives in water, and then add LiNi 0.5 Mn 1.5 O4 material, and stirring evenly to obtain a composite slurry, wherein the second additive is poly(3,4-ethylenedioxythiophene):polystyrene sulfonate; (4) introducing nitrogen into a high-temperature and high-pressure reactor containing the composite slurry, heating and pressurizing the slurry under stirring to change the slurry into a supercritical state, and cooling and releasing the pressure after the reaction in this state to obtain a post-reaction slurry; (5) After the reaction, the slurry is filtered and dried to obtain the product.
2. The method for preparing the lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: In step (1), the mixing time is 1 to 12 hours.
3. The method for preparing the lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: In step (1), the manganese source is at least one of manganese dioxide, manganese carbonate, and manganese tetroxide, the nickel source is nickel acetate, the lithium source is lithium carbonate, and the additive one is at least one of magnesium carbonate, aluminum hydroxide, chromium oxide, titanium oxide, niobium oxide, and aluminum fluoride, and the amount of additive one added is 1% to 5% of the total mass of the nickel source and the manganese source.
4. The method for preparing the lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: In step (2), the drying temperature is 120° C. and the drying time is 12 h.
5. The method for preparing the lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: In step (3), the manganese source is at least one of manganese sulfate, manganese nitrate, and manganese acetate; the iron source is at least one of iron nitrate and iron sulfate; the lithium source is at least one of lithium carbonate and lithium hydroxide; the phosphorus source is at least one of phosphoric acid and diammonium phosphate; and the carbon source is at least one of glucose and sucrose.
6. The method for preparing the lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: In step (2), the temperature is raised from room temperature to 800°C to 900°C at a rate of 4 to 6°C / min, sintered for 8h to 16h, and then annealed to 600°C to 700°C and kept at that temperature for 4h to 8h.
7. The method for preparing the lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: In step (3), LiMn x Fe (1-x) The mass of PO4 accounts for the mass of LiNi 0.5 Mn 1.5 O4 material and LiMn x Fe (1-x) 5% to 20% of the total mass of PO4.
8. The method for preparing the lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: In step (3), the molar number of additive 2 is 1% to 5% of the total molar number of Mn and Fe in the manganese source and the iron source.
9. The method for preparing the lithium iron manganese phosphate modified high-voltage lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: In step (4), the temperature of the reactor is 350-400°C, the pressure is 25-30Mpa, and the time is 20-30min.
10. A lithium manganese iron phosphate modified high-voltage lithium nickel manganese oxide positive electrode material, characterized in that: The invention is prepared by the preparation method according to claims 1 to 9.