Small-particle-size ultrahigh-nickel multi-element positive electrode material precursor and preparation method thereof
Adjust the precipitation reaction environment through the pH self-driven co-precipitation method, which solves the problems of crystallinity and sphericality of the precursor of ultra-high nickel ternary positive electrode material in traditional methods, and achieves excellent density and sphericality of small-particle material, reducing the Preparation cost and avoid pH instability.
Patent Information
- Application Number
- CN202411005481.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-25
AI Technical Summary
When preparing ultra-high nickel ternary positive electrode material precursor, traditional co-precipitation methods can easily lead to poor crystallinity, poor spherical shape and loose porosity problems, and high solids content systems can easily cause the pH meter diaphragm pores to be blocked, resulting in pH instability. Influences material performance.
The pH self-driven co-precipitation method is adopted to adjust the pH value and ammonia concentration of the base liquid, control the feeding speed of the salt material, ensure that the supersaturation of the precipitate gradually decreases, slowly transitions to the growth state, reduces fluctuations in the reaction environment, and improves the material crystallinity and sphericality.
The compactness and sphericality of the precursor of the nickel multivariate cathode material with ultra-high particle size are achieved, which reduces the cost of material preparation, avoids the pH value instability caused by pH meter blockage failure, and improves the performance stability of the material.
Smart Images

Figure CN118908308A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a small-particle ultra-high nickel multi-element positive electrode material precursor and a preparation method thereof. Background Art
[0002] In the ultra-high nickel ternary cathode material LiNi x Co y Mn 1-x-y Ultra-high nickel multi-element cathode materials can be formed by removing, supplementing and replacing elements on the basis of O2 (x≥0.90), so ultra-high nickel ternary cathode materials are used as an example for explanation. Ultra-high nickel ternary cathode materials have a high theoretical capacity (273mAh / g-285mAh / g) and an actual capacity of more than 220mAh / g, which will directly promote the improvement of the energy density of the battery system. In addition, the cobalt content of the material is low, which can minimize the cost and promote the industrial application of materials.
[0003] Material preparation methods include co-precipitation, high-temperature solid phase method, sol-gel method, hydrothermal method and spray pyrolysis method. From the perspective of actual production, in order to improve material output and batch quality, laboratories and industry often use co-precipitation method to prepare ultra-high nickel ternary cathode material precursor Ni x Co y Mn 1-x-y (OH)2(x≥0.90), and then lithium salt is added and sintered in a pure oxygen atmosphere. The layered structure of the precursor undergoes a topological transformation to obtain an ultra-high nickel ternary positive electrode material. The physical and chemical properties of the precursor material, such as crystallinity, grain morphology, particle size, and sphericity, directly determine the performance of the ternary positive electrode material. However, the high nickel, low cobalt, and low manganese components make the precursor extremely sensitive to environmental changes during the co-precipitation process. There are large differences in the growth parameters of precursors with different chemical compositions or even different particle sizes of the same chemical composition, and it is easy to obtain precursors with poor crystallinity, poor sphericity, and loose porous properties. Therefore, optimizing the co-precipitation reaction parameters is crucial for the preparation of precursor materials with excellent physical and chemical properties.
[0004] The ultra-high nickel ternary cathode material has a rapid decline in battery performance due to the drastic surface and interface structural degradation, and single crystalization is an important method to improve the stability of the material's bulk and interface structure. It can effectively alleviate the stress concentration and crack initiation caused by anisotropic lattice changes during lithium storage, inhibit the electrolyte from penetrating into the material's bulk to cause further surface and interface structural degradation, and greatly improve the material's capacity retention rate. Studies have shown that single crystal materials and small-particle polycrystalline materials have more advantages than conventional polycrystalline materials in terms of matching with solid-state battery systems, gas production, and heat generation.
[0005] Single crystal materials and small-particle polycrystalline materials evolve from small-particle precursors through different sintering processes. The preparation of small-particle ultra-high nickel ternary cathode material precursors requires precise control of the critical point of the equilibrium of the thermodynamic and kinetic processes of nucleation and growth, control of the size of the secondary particle condensation growth in the initial stage of the reaction, and then rapid increase of the solid content to end the condensation growth process and turn to independent nucleation and surface epitaxy and adsorption growth. However, this process will cause the pores (rings) of the online pH meter diaphragm to be blocked, causing the pH value of the system to become unstable. Due to the high nickel and low manganese components of the ultra-high nickel small-particle precursor, it is extremely sensitive to changes in the co-precipitation reaction environment during the growth process. As the precursor particle size increases, the optimal co-precipitation parameters are not constant, and the supersaturation of the precipitate needs to be gradually reduced to meet the requirements of epitaxial growth. Therefore, the traditional method of using constant co-precipitation parameters is prone to poor crystallinity and loose porous precursors, while the traditional method of distinguishing the nucleation and growth process parameters is prone to rapid condensation of the crystal nuclei of the ultra-high nickel small-particle precursor, resulting in precursor particle agglomeration and poor sphericity. Summary of the invention
[0006] In view of this, the present invention provides a small-particle ultra-high nickel multi-element cathode material precursor and a preparation method thereof. The present invention adopts a pH self-driven co-precipitation method to prepare a small-particle ultra-high nickel multi-element cathode material precursor. During the preparation process, the pH value is slowly reduced, so that the supersaturation of the precipitate is gradually reduced, and the nucleation state is slowly transitioned to the growth state, which reduces the fluctuation of the reaction environment and improves the crystallinity, tap density and sphericity of the material.
[0007] The present invention is achieved by adopting the following technical solutions:
[0008] A small-particle ultra-high nickel multi-element positive electrode material precursor, characterized in that the chemical formula of the small-particle ultra-high nickel multi-element positive electrode material precursor is as follows:
[0009] Ni a B b C c D d (OH)2,
[0010] Wherein, B is Fe or Co, C is Mn, and D is one of Al, Na, Mg, K, Ca, Ti, Nb, and Zr;
[0011] 90at.%≤a≤98at.%, 0.1at.%≤b≤10at.%, 0.1at.%≤c≤10at.%, 0at.%≤d≤10at.%, a+b+c+d=1.
[0012] Another object of the present invention is to provide a method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor, comprising the following steps:
[0013] (1) weighing nickel salt, B salt, C salt and D salt in proportion, and dissolving them in water to prepare a mixed metal salt solution;
[0014] (2) adding an ammonia solution as a base liquid to a reactor, introducing nitrogen, setting the speed of the stirrer to 800 r / min-1200 r / min, stirring evenly and heating to 50° C.-60° C., adding an alkali solution to adjust the pH value of the base liquid to 11.0-11.8, and then adding the mixed metal salt solution and the complexing agent at the same time to perform a precipitation reaction, adjusting the feed rates of the alkali solution and the mixed metal salt solution during the reaction so that the ratio of the amount of hydroxide to the amount of salt entering the reactor per unit time is 2:1, and finally filtering to obtain a precipitate;
[0015] (3) The precipitate obtained in step (2) is washed with deionized water and then filtered until the pH value of the filtrate is neutral, dried at 90° C.-150° C. for 12 h-24 h, and sieved to remove magnetism to obtain a small-particle ultra-high nickel multi-element positive electrode material precursor.
[0016] Furthermore, the nickel salt includes nickel sulfate, nickel carbonate, nickel oxalate, nickel acetate and hydrates thereof.
[0017] Furthermore, the B salt is ferric sulfate, ferric nitrate, ferric chloride, ferrous carbonate, ferric citrate, cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt oxalate and hydrates thereof.
[0018] Furthermore, the C salt is manganese sulfate, manganese nitrate, manganese carbonate, manganese chloride and hydrates thereof.
[0019] Furthermore, the D salt is sulfate, carbonate, nitrate, oxalate and hydrate thereof containing Al, Na, Mg, K, Ca, Ti, Nb and Zr elements.
[0020] Preferably, the molar concentration of the mixed metal salt solution is 1 mol / L-4 mol / L.
[0021] Preferably, the base liquid is an aqueous ammonia solution with a molar concentration of 0.3 mol / L-1.1 mol / L.
[0022] Preferably, the volume of the bottom liquid accounts for 1 / 3-1 / 2 of the total volume of the reactor.
[0023] Preferably, the alkaline solution is a NaOH solution with a molar concentration of 4 mol / L-8 mol / L.
[0024] Preferably, the complexing agent is an aqueous ammonia solution with a molar concentration of 4 mol / L-8 mol / L.
[0025] Furthermore, before the precipitation reaction in step (2), the mixed metal salt solution, the base solution (ammonia solution) and the alkaline solution (NaOH solution) need to be filtered to remove undissolved solid impurities.
[0026] Preferably, the feed rate of the mixed metal salt solution is 0.5 mL / min-20.0 mL / min.
[0027] Preferably, the feed rate of the alkaline solution is 0.3 mL / min-40.0 mL / min.
[0028] Preferably, the feeding rate of the complexing agent is 0.2 mL / min-25.0 mL / min.
[0029] Preferably, the ammonia concentration is maintained at 0.3 mol / L-1.1 mol / L during the precipitation reaction.
[0030] The present invention adopts a pH self-driven co-precipitation method to prepare a small-particle ultra-high nickel multi-element positive electrode material precursor. The present invention adjusts the bottom liquid to reach a preset pH value and ammonia concentration, determines the salt feed rate, and then adjusts the feed rate of the alkaline solution so that the amount of hydroxyl radicals entering the reactor per unit time is exactly twice the amount of salt, that is, the precursor chemical formula coefficient ratio is satisfied, so that the salt and alkali entering the reaction system per unit time are just completely precipitated, and then the complexing agent feed rate is adjusted to maintain the ammonia concentration during the reaction process, so that the ammonia concentration during the reaction process remains unchanged, and finally the nucleation and growth of the small-particle ultra-high nickel multi-element positive electrode material precursor are completed, so that the primary particle morphology and the secondary particle size are dynamically adjusted by the bottom liquid pH value and ammonia concentration.
[0031] The primary particles of the small-particle ultra-high nickel multi-element positive electrode material precursor of the present invention have obvious layered structure, dense secondary particles, excellent sphericity, concentrated particle size distribution, a span of less than 1.2, and an average secondary particle size D50 of 2μm-6μm.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1. The present invention adopts a pH self-driven co-precipitation method to prepare a small-particle ultra-high nickel multi-element positive electrode material precursor. During the preparation process, the pH value is slowly reduced, so that the supersaturation of the precipitate gradually decreases, and it slowly transitions from the nucleation state to the growth state, reducing the fluctuation of the reaction environment, which is beneficial to improving the crystallinity, tap density and sphericity of the material.
[0034] 2. Small-particle precursors require a high solid content in the reaction system to reduce the growth rate of the precursor particle size. However, a high-solid content system can easily cause the pH meter diaphragm hole (ring) to become clogged, causing the pH meter to fail and triggering the pH value of the reaction system to become unstable. The present invention only needs to control the pH value of the bottom liquid before the reaction starts so that the pH value reaches a preset value. After the mixed metal salt solution and the complexing agent enter, there is no need to keep the pH value constant. When the alkaline solution is fed, the pH meter automatically controls the speed to be constant, thereby avoiding the pH value of the reaction system to become unstable due to the blockage and failure of the pH meter in a high-solid content system.
[0035] 3. The traditional method requires the online pH meter to be isolated and cleaned during the reaction process to maintain a constant pH value of the reaction system. The present invention does not require the pH meter to be cleaned during the reaction process, which can greatly reduce the cost of material preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The small-sized Ni prepared in Example 1 of the present invention 0.92 Co 0.04 Mn 0.04 Scanning electron microscopy (SEM) test image of (OH)2 precursor;
[0037] Figure 2 The small-sized Ni prepared in Example 1 of the present invention 0.92 Co 0.04 Mn 0.04 Particle size distribution diagram of (OH)2 precursor;
[0038] Figure 3 The small-sized Ni prepared in Example 2 of the present invention 0.92 Co 0.04 Mn 0.04 SEM test image of (OH)2 precursor;
[0039] Figure 4 The small-sized Ni prepared in Example 2 of the present invention 0.92 Co 0.04 Mn 0.04 Particle size distribution diagram of (OH)2 precursor;
[0040] Figure 5 The small-sized Ni prepared in Example 3 of the present invention 0.92 Co 0.04 Mn 0.04 SEM test image of (OH)2 precursor;
[0041] Figure 6 The small-sized Ni prepared in Example 3 of the present invention 0.92 Co 0.04 Mn 0.04 Particle size distribution diagram of (OH)2 precursor;
[0042] Figure 7 The small-sized Ni prepared in Example 3 of the present invention 0.92 Co 0.04 Mn 0.04 X-ray diffraction (XRD) test pattern of (OH)2 precursor;
[0043] Figure 8 The small-sized Ni prepared in Example 4 of the present invention 0.950 Fe 0.025 Mn 0.025 SEM test image of (OH)2 precursor;
[0044] Fig. 9 The small-sized Ni prepared in Example 4 of the present invention 0.950 Fe 0.025 Mn 0.025 Particle size distribution diagram of (OH)2 precursor;
[0045] Fig.10 The small-sized Ni prepared in Example 5 of the present invention 0.90 Co 0.03 Mn 0.05 Nb 0.02 SEM test image of (OH)2 precursor;
[0046] Fig.11 The small-sized Ni prepared in Example 5 of the present invention 0.90 Co 0.03 Mn 0.05 Nb 0.02 Particle size distribution of (OH)2 precursor.
[0047] Fig.12 The small-sized Ni prepared in Comparative Example 1 of the present invention 0.92 Co 0.04 Mn 0.04 SEM test image of (OH)2 precursor;
[0048] Fig.13 The small-sized Ni prepared in Comparative Example 1 of the present invention 0.92 Co 0.04 Mn 0.04 Particle size distribution of (OH)2 precursor. DETAILED DESCRIPTION
[0049] The present invention will be further described below in conjunction with the embodiments.
[0050] Example 1
[0051] A method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor comprises the following steps:
[0052] (1) nickel sulfate hexahydrate (NiSO4·6H2O), cobalt sulfate heptahydrate (CoSO4·7H2O), and manganese sulfate monohydrate (MnSO4·H2O) were weighed according to the metal molar ratio of 92:4:4, and prepared into a 2 mol / L mixed metal salt solution, and an ammonia solution with a molar concentration of 6 mol / L was used as a complexing agent, and a NaOH solution with a molar concentration of 6 mol / L was used as an alkaline solution, and the above solution was filtered to remove solid impurities and precipitates;
[0053] (2) Add an ammonia solution with a molar concentration of 0.5 mol / L as the bottom liquid to the reactor, and the volume of the bottom liquid is 1 / 3 of the volume of the reactor. Then, introduce nitrogen to replace the air in the reactor, stir evenly, and heat to 55°C at a stirring speed of 1000 r / min. After the temperature stabilizes, turn on the alkali pump to add NaOH solution to adjust the pH value of the bottom liquid to 11.2. At the same time, turn on the salt pump and ammonia pump to add a mixed metal salt solution and a complexing agent. Adjust the feed rate of the alkali pump to 11.63 mL / min, the feed rate of the salt pump to 17.45 mL / min, and the feed rate of the ammonia pump to 5.88 mL / min, and react for 30 hours.
[0054] (3) The product obtained in step (2) was thoroughly washed with deionized water and filtered until the pH value of the filtrate was neutral, and the filter cake was placed in a drying oven at 100° C. and dried for 24 h. After sieving and removing the magnetism, a small-particle ultra-high nickel multi-element positive electrode material precursor Ni 0.92 Co 0.04 Mn 0.04 (OH)2.
[0055] The small-sized Ni prepared in Example 1 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor was subjected to SEM test (FlexSEM1000II), and the test image is as follows Figure 1 As shown; when the base liquid concentration is 0.5 mol / L, the precursor morphology after pH self-driven growth is spherical secondary particles assembled from layered lamellar primary particles. The material has excellent sphericity and high density.
[0056] The small-sized Ni prepared in Example 1 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor was tested for particle size (Bettersize2600), and the particle size distribution diagram is shown in Figure 2 As shown; when the base liquid concentration is 0.5 mol / L, the precursor particle size D50 after pH self-driven growth is 2.709 μm, the particle size span is 0.901, and there are no obvious impurity peaks except the main peak in the particle size distribution diagram. The material particle size is small and the distribution is concentrated.
[0057] Example 2
[0058] A method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor comprises the following steps:
[0059] (1) nickel sulfate hexahydrate (NiSO4·6H2O), cobalt sulfate heptahydrate (CoSO4·7H2O), and manganese sulfate monohydrate (MnSO4·H2O) were weighed according to the metal molar ratio of 92:4:4, and prepared into a 2 mol / L mixed metal salt solution, and an ammonia solution with a molar concentration of 6 mol / L was used as a complexing agent, and a NaOH solution with a molar concentration of 6 mol / L was used as an alkaline solution, and the above solution was filtered to remove solid impurities and precipitates;
[0060] (2) Add an ammonia solution with a molar concentration of 0.3 mol / L as the bottom liquid to the reactor, and the volume of the bottom liquid is 1 / 2 of the volume of the reactor. Then, introduce nitrogen to replace the air in the reactor, stir evenly, and heat to 55°C at a stirring speed of 1000 r / min. After the temperature stabilizes, turn on the alkali pump to add NaOH solution to adjust the pH value of the bottom liquid to 11.2. At the same time, turn on the salt pump and ammonia pump to add a mixed metal salt solution and a complexing agent. Adjust the feed rate of the alkali pump to 11.63 mL / min, the feed rate of the salt pump to 17.45 mL / min, and the feed rate of the ammonia pump to 5.88 mL / min, and react for 30 hours.
[0061] (3) The product obtained in step (2) was thoroughly washed with deionized water and filtered until the pH value of the filtrate was neutral, and the filter cake was placed in a drying oven at 100° C. and dried for 24 h. After sieving and removing the magnetism, a small-particle ultra-high nickel multi-element positive electrode material precursor Ni 0.92 Co 0.04 Mn 0.04 (OH)2.
[0062] The small-sized Ni prepared in Example 2 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor was subjected to SEM test (FlexSEM1000II), and the test image is as follows Figure 3 As shown; when the base solution concentration is 0.3 mol / L, the precursor morphology after pH self-driven growth is spherical secondary particles assembled from layered short lamellar primary particles. The material has excellent sphericity and high density. Compared with the base solution concentration of 0.5 mol / L, the primary particle size is reduced.
[0063] The small-sized Ni prepared in Example 2 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor was tested for particle size (Bettersize2600), and the particle size distribution diagram is shown in Figure 4As shown; when the bottom liquid concentration is 0.3 mol / L, the precursor particle size D50 after pH self-driven growth is 2.880 μm, and the particle size span is 1.032. Due to the low bottom liquid ammonia concentration and the long duration of the nucleation process, small particle size peaks appear in the particle size distribution diagram, and the overall particle size distribution is relatively concentrated.
[0064] Example 3
[0065] A method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor comprises the following steps:
[0066] (1) nickel sulfate hexahydrate (NiSO4·6H2O), cobalt sulfate heptahydrate (CoSO4·7H2O), and manganese sulfate monohydrate (MnSO4·H2O) were weighed according to the metal molar ratio of 92:4:4, and prepared into a 2 mol / L mixed metal salt solution, and an ammonia solution with a molar concentration of 6 mol / L was used as a complexing agent, and a NaOH solution with a molar concentration of 6 mol / L was used as an alkaline solution, and the above solution was filtered to remove solid impurities and precipitates;
[0067] (2) Add an ammonia solution with a molar concentration of 1.1 mol / L as the bottom liquid to the reactor, and the volume of the bottom liquid is 1 / 3 of the volume of the reactor. Then, introduce nitrogen to replace the air in the reactor, stir evenly, and heat to 55°C at a stirring speed of 1000 r / min. After the temperature stabilizes, turn on the alkali pump to add NaOH solution to adjust the pH value of the bottom liquid to 11.2. At the same time, turn on the salt pump and ammonia pump to add a mixed metal salt solution and a complexing agent. Adjust the feed rate of the alkali pump to 11.63 mL / min, the feed rate of the salt pump to 17.45 mL / min, and the feed rate of the ammonia pump to 5.88 mL / min, and react for 30 hours.
[0068] (3) The product obtained in step (2) was thoroughly washed with deionized water and filtered until the pH value of the filtrate was neutral, and the filter cake was placed in a drying oven at 100° C. and dried for 24 h. After sieving and removing the magnetism, a small-particle ultra-high nickel multi-element positive electrode material precursor Ni 0.92 Co 0.04 Mn 0.04 (OH)2.
[0069] The small-sized Ni prepared in Example 3 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor was subjected to SEM test (FlexSEM1000II), and the test image is as follows Figure 5 As shown; when the base solution concentration is 1.1 mol / L, the precursor morphology after pH self-driven growth is spherical secondary particles assembled from layered blocky primary particles. The material has excellent sphericity and high density. Compared with the base solution concentration of 0.5 mol / L, the primary particle size is significantly increased.
[0070] The small-sized Ni prepared in Example 3 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor was tested for particle size (Bettersize2600), and the particle size distribution diagram is shown in Figure 6 As shown; when the base liquid concentration is 1.1 mol / L, the precursor particle size D50 after pH self-driven growth is 4.649 μm, the particle size span is 0.580, and the high base liquid ammonia concentration significantly increases the secondary particle size. In the particle size distribution diagram, there are no other peaks except the main peak, and the material particle size is small and concentrated.
[0071] The small-sized Ni prepared in Example 3 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor was subjected to XRD test (Japan Rigaku SmartLab), and the test spectrum is as follows Figure 7 As shown; the diffraction peak in the XRD spectrum basically corresponds to Ni(OH)2. 2+ The ionic radius is larger than Co 2+ and Mn 2+ , so the precursor Ni 0.92 Co 0.04 Mn 0.04 The diffraction peak of (OH)2 is shifted to a high angle relative to the Ni(OH)2 standard card, the diffraction pattern has no impurity peaks, and the material has good crystallinity.
[0072] Example 4
[0073] A method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor comprises the following steps:
[0074] (1) nickel sulfate hexahydrate (NiSO4·6H2O), ferrous sulfate heptahydrate (FeSO4·7H2O), and manganese sulfate monohydrate (MnSO4·H2O) were weighed according to the molar ratio of metal substances of 95:2.5:2.5, and prepared into a 2 mol / L mixed metal salt solution, and an ammonia solution with a molar concentration of 6 mol / L was used as a complexing agent, and a NaOH solution with a molar concentration of 6 mol / L was used as an alkaline solution, respectively, and the above solutions were filtered to remove solid impurities and precipitates;
[0075] (2) Add an ammonia solution with a molar concentration of 1.1 mol / L as the bottom liquid to the reactor, and the volume of the bottom liquid is 1 / 3 of the volume of the reactor. Then, introduce nitrogen to replace the air in the reactor, stir evenly, and heat to 55°C at a stirring speed of 1000 r / min. After the temperature stabilizes, turn on the alkali pump to add NaOH solution to adjust the pH value of the bottom liquid to 11.4. At the same time, turn on the salt pump and ammonia pump to add a mixed metal salt solution and a complexing agent. Adjust the feed rate of the alkali pump to 3.50 mL / min, the feed rate of the salt pump to 5.24 mL / min, and the feed rate of the ammonia pump to 1.55 mL / min. React for 30 hours.
[0076] (3) The product obtained in step (2) was thoroughly washed with deionized water and filtered until the pH value of the filtrate was neutral, and the filter cake was placed in a drying oven at 100° C. and dried for 24 h. After sieving and removing the magnetism, a small-particle ultra-high nickel multi-element positive electrode material precursor Ni 0.950 Fe 0.025 Mn 0.025 (OH)2.
[0077] The small-sized Ni prepared in Example 4 0.950 Fe 0.025 Mn 0.025 The (OH)2 precursor was subjected to SEM test (FlexSEM1000II), and the test image is as follows Figure 8 As shown; the morphology of the precursor after pH self-driven growth is spherical secondary particles assembled from layered spindle-shaped primary particles. The material has excellent sphericity and high density.
[0078] The small-sized Ni prepared in Example 4 0.950 Fe 0.025 Mn 0.025 The (OH)2 precursor was tested for particle size (Bettersize2600), and the particle size distribution diagram is shown in Fig. 9 As shown; the precursor particle size D50 after pH self-driven growth is 4.318μm, the particle size span is 0.592, and there are no other peaks except the main peak in the particle size distribution diagram. The material particle size is small and the distribution is concentrated, indicating that the pH self-driven co-precipitation method is also suitable for the synthesis of small-particle ultra-high nickel cobalt-free multi-element positive electrode material precursors.
[0079] Example 5
[0080] A method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor comprises the following steps:
[0081] (1) nickel sulfate hexahydrate (NiSO4·6H2O), cobalt sulfate heptahydrate (CoSO4·7H2O), manganese sulfate monohydrate (MnSO4·H2O) and ammonium niobate oxalate hydrate (C4H4NNbO9·nH2O) were weighed according to the molar ratio of metal substances of 90:3:5:2, and prepared into a 1 mol / L mixed metal salt solution, and an ammonia solution with a molar concentration of 4 mol / L was used as a complexing agent, and a NaOH solution with a molar concentration of 4 mol / L was used as an alkaline solution, and the above solution was filtered to remove solid impurities and precipitates;
[0082] (2) Add an ammonia solution with a molar concentration of 0.8 mol / L as the bottom liquid to the reactor, and the volume of the bottom liquid is 1 / 3 of the volume of the reactor. Then, introduce nitrogen to replace the air in the reactor, stir evenly, and heat to 57°C at a stirring speed of 800 r / min. After the temperature stabilizes, turn on the alkali pump to add NaOH solution to adjust the pH value of the bottom liquid to 11.5. At the same time, turn on the salt pump and ammonia pump to add a mixed metal salt solution and a complexing agent. Adjust the feed rate of the alkali pump to 1.31 mL / min, the feed rate of the salt pump to 2.62 mL / min, and the feed rate of the ammonia pump to 0.98 mL / min. React for 40 hours.
[0083] (3) The product obtained in step (2) was thoroughly washed with deionized water and filtered until the pH value of the filtrate was neutral, and the filter cake was placed in a drying oven at 120° C. and dried for 24 h. After sieving and removing the magnetism, a small-particle ultra-high nickel multi-element positive electrode material precursor Ni 0.90 Co 0.03 Mn 0.05 Nb 0.02 (OH)2.
[0084] The small-sized Ni prepared in Example 5 0.90 Co 0.03 Mn 0.05 Nb 0.02 The (OH)2 precursor was subjected to SEM test (FlexSEM1000II), and the test image is as follows Fig.10 As shown; the morphology of the quaternary material precursor that undergoes pH self-driven growth is spherical secondary particles assembled from short spindle primary particles. The material has excellent sphericity and high density.
[0085] The small-sized Ni prepared in Example 5 0.90 Co 0.03 Mn 0.05 Nb 0.02 The (OH)2 precursor was tested for particle size (Bettersize2600), and the particle size distribution diagram is shown in Fig.11As shown; when the base solution concentration is 0.8 mol / L, the precursor particle size D50 after pH self-driven growth is 4.455 μm, the particle size span is 0.584, and the overall particle size distribution is relatively concentrated.
[0086] Comparative Example 1
[0087] Comparative Example 1 maintained a constant pH value during the entire reaction process, and the other parameters remained the same as those of Example 1, specifically comprising the following steps:
[0088] (1) nickel sulfate hexahydrate (NiSO4·6H2O), cobalt sulfate heptahydrate (CoSO4·7H2O), and manganese sulfate monohydrate (MnSO4·H2O) were weighed according to the metal molar ratio of 92:4:4, and prepared into a 2 mol / L mixed metal salt solution, and an ammonia solution with a molar concentration of 6 mol / L was used as a complexing agent, and a NaOH solution with a molar concentration of 6 mol / L was used as an alkaline solution, respectively, and the above solutions were filtered to remove solid impurities and precipitates;
[0089] (2) Add an ammonia solution with a molar concentration of 0.5 mol / L as a base liquid to the reactor, and the volume of the base liquid is 1 / 3 of the volume of the reactor. Then, introduce nitrogen to replace the air in the reactor, stir evenly, and heat to 55°C at a stirring speed of 1000 r / min. After the temperature stabilizes, turn on the alkali pump to add NaOH solution, and use a PID program control system to control the alkali pump feed rate to control the pH value of the reaction system to 11.2. At the same time, turn on the salt pump and ammonia pump to add a mixed metal salt solution and a complexing agent, adjust the salt pump feed rate to 17.45 mL / min, and the ammonia pump feed rate to 5.88 mL / min, and react for 30 hours.
[0090] (3) The product obtained in step (2) was thoroughly washed with deionized water and filtered until the pH value of the filtrate was neutral, and the filter cake was placed in a drying oven at 100° C. and dried for 24 h. After sieving and removing the magnetism, a small-particle ultra-high nickel multi-element positive electrode material precursor Ni 0.92 Co 0.04 Mn 0.04 (OH)2.
[0091] The small-sized Ni prepared in Comparative Example 1 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor was subjected to SEM test (FlexSEM1000II), and the test image is as follows Fig.12 As shown in the figure, when a constant pH value is maintained during the reaction, the supersaturation of the precipitate is high, and the precursor is always in a nucleation state, resulting in incomplete development of the primary particles of the final product and missing morphology. The secondary particles are irregular loose agglomerates with low tap density, poor crystallinity and sphericity.
[0092] The small-sized Ni prepared in Comparative Example 1 0.92 Co 0.04 Mn 0.04 The (OH)2 precursor was tested for particle size (Bettersize2600), and the particle size distribution diagram is shown in Fig.13 As shown; due to maintaining a constant pH value, the secondary particles show irregular loose agglomeration, resulting in a large span of particle size distribution. Under the cutting action of the stirring paddle, the loose small particles are peeled off from the surface of the secondary particles, and small particle size peaks appear in the particle size distribution diagram.
[0093] Through the analysis of the results of Example 1 and Comparative Example 1, it is found that maintaining a constant pH value cannot simultaneously meet the requirements of the nucleation and growth processes of the small-particle ultra-high nickel multi-element positive electrode material precursor. Instead, the pH value is slowly reduced by relying on the increase in the liquid phase volume in the reactor, that is, the pH self-driven process can slowly transition from the nucleation state to the growth state, reducing the fluctuation of the reaction environment, and thereby obtaining a small-particle precursor material with high tap density, high crystallinity and excellent sphericity, reflecting the necessity of pH self-driving.
[0094] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A small-particle ultra-high nickel multi-element positive electrode material precursor, characterized in that: The chemical formula of the small-particle ultra-high nickel multi-element cathode material precursor is as follows: Ni a B b C c D d (OH)2, Wherein, B is Fe or Co, C is Mn, and D is one of Al, Na, Mg, K, Ca, Ti, Nb, and Zr; 90at.%≤a≤98at.%, 0.1at.%≤b≤10at.%, 0.1at.%≤c≤10at.%, 0at.%≤d≤10at.%, a+b+c+d=1.
2. The method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor according to claim 1, characterized in that: The following steps are involved: (1) weighing nickel salt, B salt, C salt and D salt in proportion, and dissolving them in water to prepare a mixed metal salt solution; (2) adding an ammonia solution as a base liquid to a reactor, introducing nitrogen, setting the speed of the stirrer to 800 r / min-1200 r / min, stirring evenly and heating to 50° C.-60° C., adding an alkali solution to adjust the pH value of the base liquid to 11.0-11.8, and then adding the mixed metal salt solution and the complexing agent at the same time to perform a precipitation reaction, adjusting the feed rates of the alkali solution and the mixed metal salt solution during the reaction so that the ratio of the amount of hydroxide to the amount of salt entering the reactor per unit time is 2:1, and finally filtering to obtain a precipitate; (3) The precipitate obtained in step (2) is washed with deionized water and then filtered until the pH value of the filtrate is neutral, dried at 90° C.-150° C. for 12 h-24 h, and sieved to remove magnetism to obtain a small-particle ultra-high nickel multi-element positive electrode material precursor.
3. The method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor according to claim 2, characterized in that: The nickel salts include nickel sulfate, nickel carbonate, nickel oxalate, nickel acetate and hydrates thereof; the B salts include ferric sulfate, ferric nitrate, ferric chloride, ferrous carbonate, ferric citrate, cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt oxalate and hydrates thereof; the C salts include manganese sulfate, manganese nitrate, manganese carbonate, manganese chloride and hydrates thereof; the D salts include sulfates, carbonates, nitrates, oxalates and hydrates thereof containing elements such as Al, Na, Mg, K, Ca, Ti, Nb and Zr.
4. The method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor according to claim 2, characterized in that: The molar concentration of the mixed metal salt solution is 1 mol / L-4 mol / L.
5. The method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor according to claim 2, characterized in that: The bottom liquid is an ammonia solution with a molar concentration of 0.3 mol / L-1.1 mol / L; the volume of the bottom liquid accounts for 1 / 3-1 / 2 of the total volume of the reactor.
6. The method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor according to claim 2, characterized in that: The alkaline solution is a NaOH solution with a molar concentration of 4 mol / L-8 mol / L; the complexing agent is an ammonia solution with a molar concentration of 4 mol / L-8 mol / L.
7. The method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor according to claim 2, characterized in that: The feed rate of the alkaline solution is 0.3 mL / min-40.0 mL / min.
8. The method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor according to claim 2, characterized in that: The feeding rate of the mixed metal salt solution is 0.5 mL / min-20.0 mL / min.
9. The method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor according to claim 2, characterized in that: The feeding rate of the complexing agent is 0.2 mL / min-25.0 mL / min.
10. The method for preparing a small-particle ultra-high nickel multi-element positive electrode material precursor according to claim 2, characterized in that: During the precipitation reaction, the ammonia concentration is maintained at 0.3 mol / L-1.1 mol / L.
Citation Information
Patent Citations
Preparation method of small-particle size ternary positive material precursor
CN107915263A
High-performance small-particle-size ternary positive electrode material precursor and preparation method thereof
CN108365214A
High-nickel lithium ion positive electrode material and preparation method thereof
CN110034297A
Preparation method of high-nickel ternary precursor washed by alkaline water
CN114057239A
Preparation method of high-nickel ternary positive electrode precursor
CN114655998A