Alkali reducing agent with preservative effect as well as preparation method and application of alkali reducing agent
By using a specially formulated alkali-reducing agent, the problems of alkali reduction and corrosion prevention in boiler water treatment are solved through the modification of active silica and the synergistic effect of components, achieving efficient scale prevention, corrosion prevention and energy saving.
Patent Information
- Application Number
- CN202411041637.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Existing boiler water treatment agents have insufficient synergistic effects in reducing boiler water alkalinity and preventing corrosion, resulting in high boiler water treatment costs and insignificant effects.
The alkali-reducing agent, formulated with specific ingredients including active silica, corrosion and scale inhibitors, cellulose ether, ferrous sulfate, sodium salt of naphthalenesulfonic acid formaldehyde condensate, and ethylenediaminetetraacetic acid, enhances corrosion prevention, scale prevention, and alkali reduction effects through surface modification and synergistic effects of its components.
It effectively reduces alkalinity, scale, and corrosion in boiler water, and reduces sewage discharge, significantly lowering water treatment costs and improving the safety and stability of boiler operation.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of water quality additives, and particularly relates to an alkali reducing agent with antiseptic effect and a preparation method and application thereof. Background Art
[0002] The steam boiler system consists of three parts: feed water, boiler body and steam-condensate. After long-term operation, the boiler feed water system and steam-condensate system have serious corrosion phenomena. The corrosion products are brought into the boiler, causing scaling and corrosion of the boiler, which brings hidden dangers to the safe and stable operation of the boiler. Due to the influence of changes in boiler water sources, the alkalinity of boiler water increases, especially in the evaporation tubes with high heat loads. If local overheating occurs, the area will form a concentrated alkaline area due to the high concentration of boiler water, so that the protective film on the metal surface will dissolve and lose its protective effect, which may cause alkaline corrosion and stress corrosion cracking of water-cooled wall tubes; it may also cause foaming in boiler water and affect steam quality. Boiler water treatment can be divided into external treatment and internal treatment. Internal treatment mainly uses chemical agents to reduce alkali, adjust pH value, and inhibit corrosion and scale in the boiler water system.
[0003] The invention patent with application number 202010121888.X discloses a low-pressure boiler phosphorus-free composite cylinder cleaning agent and a preparation method. The invention consists of a deoxidizer component, a corrosion inhibitor component, a scale inhibitor component, a pH stabilizer component, etc. The weight percentage of each component is: deoxidizer component: 5%-20%, corrosion inhibitor component: 1%-10%, scale inhibitor component: 0.1%-10%, pH stabilizer component: 0.1%-10%, and the rest is pure water; it is widely used in water replenishment of pure water, softened water and ordinary tap water. Low-pressure steam boilers and hot water boilers can be added to the boiler make-up water to eliminate dissolved oxygen corrosion in the feed water and have a slow-release scale inhibition effect in the boiler water. At the same time, the specific neutralizing amine component can also effectively solve the corrosion problem at the condensate end, providing a one-barrel water treatment solution for low-pressure boilers. It is phosphorus-free, environmentally friendly, safe and efficient. However, when the functional water treatment agents are mixed, the synergistic effect between the components still has room for improvement. For example, the scale inhibition and alkali reduction effect. If the synergistic effect between the components can be fully utilized, the boiler water treatment cost can be effectively reduced.
[0004] In view of this, the alkali reducing agent with antiseptic effect disclosed in the present invention is particularly important. Summary of the invention
[0005] In view of the defects of the prior art, the present invention provides an alkali reducing agent with an anti-corrosion effect and a preparation method thereof. The alkali reducing agent with an anti-corrosion effect provided by the present invention is an environmentally friendly agent for boilers with excellent comprehensive performance, a reasonable and scientific formula, and synergistic synergy of various components. While effectively reducing the alkalinity of boiler water, it also plays the role of anti-scaling, anti-corrosion, steam purification, and greatly reducing the amount of boiler water sewage, and has a significant energy-saving and consumption-reducing effect.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] On one hand, the present invention provides an alkali reducing agent with an anti-corrosion effect, which comprises the following raw materials in parts by weight: 2-3 parts of active silicon dioxide, 2-2.5 parts of corrosion and scale inhibitors, 0.8-2.5 parts of cellulose ether, 0.5-1.5 parts of ferrous sulfate, 1-1.5 parts of naphthalenesulfonic acid formaldehyde condensate sodium salt and 0.5-1 part of ethylenediaminetetraacetic acid.
[0008] In some embodiments of the present invention, the preparation steps of the active silicon dioxide are as follows:
[0009] Add 10-30 wt% of inorganic alkali solution and silicon dioxide into a reactor, stir evenly, then add a coupling agent, and calcine at 120-170° C. for 1-3 hours to obtain the active silicon dioxide.
[0010] Preferably, the preparation steps of the active silicon dioxide are as follows:
[0011] Add 20 wt % of inorganic alkali solution and silicon dioxide into the reactor, stir evenly, then add coupling agent, and calcine at 145° C. for 2 hours to obtain the active silicon dioxide.
[0012] In some embodiments of the present invention, the mass ratio of the inorganic alkaline solution to silicon dioxide is (0.5-1):1.
[0013] Preferably, the mass ratio of the inorganic alkaline solution to silicon dioxide is 0.75:1.
[0014] Preferably, the inorganic alkali solution is a 20 wt % sodium hydroxide solution.
[0015] In some embodiments of the present invention, the mass ratio of the coupling agent to silicon dioxide is (0.05-0.1):1.
[0016] Preferably, the mass ratio of the coupling agent to silica is 0.075:1.
[0017] Preferably, the coupling agent is hexadecyltrimethoxysilane.
[0018] In some embodiments of the present invention, the particle size of the silicon dioxide is 20-100 mesh.
[0019] The present invention modifies silica with a specific particle size by using a coupling agent and organically modifies its surface to increase its compatibility with the organic components in the alkali reducing agent. When it is added into the alkali reducing agent system, the efficiency of its reaction with inorganic alkali to generate silicate can be accelerated. The combination of the silica with impurities such as iron oxide and manganese oxide can be utilized to form insoluble precipitates to prevent pipeline corrosion.
[0020] In some embodiments of the present invention, the corrosion and scale inhibitor is a phosphonocarboxylic acid copolymer having a number average molecular weight of 2000-4000.
[0021] The applicant selected a phosphonyl-containing carboxylic acid polymer with a number average molecular weight of 2000 to 4000 and added it to the alkali reducer system to activate the -PO(OH)2 group and -COOH group in its molecular structure, thereby destroying the lattice structure and normal growth model of the scale particles, desorbing the scale particles from the metal surface, and effectively exerting the scale inhibition and dispersibility of the carboxylic acid polymer while improving the corrosion inhibition performance of the alkali reducer system.
[0022] In some embodiments of the present invention, the alkalinity reducing agent further comprises octadecanoic acid.
[0023] In some embodiments of the present invention, the mass ratio of the corrosion inhibitor and scale inhibitor to octadecanoic acid is 1:(0.06-0.13).
[0024] Preferably, the mass ratio of the corrosion inhibitor and scale inhibitor to octadecanoic acid is 1:0.09.
[0025] The applicant reduced the surface tension of the system solution, increased the dispersion stability of the system, and increased the solubility of other components by adding a specific proportion of octadecanoic acid. At the same time, it was unexpectedly discovered that by further adjusting the mass ratio of the surfactant to the corrosion and scale inhibitor, the scale inhibition effect of the alkali reducer system was significantly improved. The possible reason is that the surfactant can promote the dissociation of the -COOH group of the corrosion and scale inhibitor to a certain extent, thereby exerting an excellent synergistic scale inhibition effect. On the other hand, it also reduces the amount of corrosion and scale inhibitor added, thereby reducing the water treatment cost.
[0026] Another aspect of the present invention provides a method for preparing an alkali reducing agent having an antiseptic effect, comprising the following steps:
[0027] Active silicon dioxide, corrosion and scale inhibitor, cellulose ether, ferrous sulfate, sodium salt of naphthalenesulfonic acid formaldehyde condensate and ethylenediaminetetraacetic acid are sequentially mixed and stirred evenly to obtain the alkali reducing agent.
[0028] In another aspect, the present invention provides application of the alkali reducing agent in a low-pressure steam boiler.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The anti-corrosion alkali reducing agent provided by the present invention is an environmentally friendly agent for boilers with excellent comprehensive performance. The formula is reasonable and scientific, and the components work together to enhance the effectiveness. While effectively reducing the alkalinity of boiler water, it also plays the role of anti-scaling, anti-corrosion, steam purification, and greatly reducing the amount of boiler water discharge, and has a significant effect of energy saving and consumption reduction;
[0031] (2) The present invention modifies silica of a specific particle size with a coupling agent and organically modifies its surface to increase its compatibility with the organic components in the alkali reducing agent. When it is added to the alkali reducing agent system, on the one hand, it accelerates its reaction with inorganic alkali to form silicate; on the other hand, it utilizes its binding effect on impurities such as iron oxide and manganese oxide to form insoluble precipitates to prevent pipeline corrosion;
[0032] (3) The alkali reducer with anti-corrosion effect provided by the present invention selects a phosphonyl-containing carboxylic acid polymer with a number average molecular weight of 2000 to 4000 and adds it to the alkali reducer system to activate the -PO(OH)2 group and -COOH group in its molecular structure, effectively exerts the scale inhibition and dispersibility of the carboxylic acid polymer, and improves the corrosion inhibition performance of the alkali reducer system;
[0033] (4) The anti-corrosion alkali reducing agent provided by the present invention also adds a specific proportion of octadecanoic acid, which significantly reduces the surface tension of the system solution, increases the dispersion stability of the system, and increases the solubility of other components in the alkali reducing agent; at the same time, by further adjusting the mass ratio of the preferred surfactant and the corrosion and scale inhibitor within a certain range, the surfactant is used to promote the dissociation of the -COOH group of the corrosion and scale inhibitor to a certain extent, thereby exerting a better synergistic scale inhibition effect, thereby simultaneously improving the scale inhibition effect of the alkali reducing agent system; on the other hand, the amount of corrosion and scale inhibitor added is reduced, thereby reducing the water treatment cost. DETAILED DESCRIPTION
[0034] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0035] If not otherwise specified, the reagents used below can be easily obtained from commercial companies, among which the phosphonocarboxylic acid copolymer, with a number average molecular weight of 3000, was purchased from Hubei Jiufenglong Chemical Co., Ltd.; naphthalenesulfonic acid formaldehyde condensate sodium salt was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.; silicon dioxide, with a particle size of 60 mesh, was purchased from Nangong Jiuxin New Material Technology Co., Ltd.; corrosion and scale inhibitor PO-600 was purchased from Shenzhen Derunfeng Industrial Co., Ltd.; cellulose ether was purchased from Henan Jinshuo Technology Co., Ltd.
[0036] Preparation Example 1
[0037] The preparation steps of the first active silicon dioxide are as follows:
[0038] 7.5 mL of 20 wt % sodium hydroxide solution and 10 g of silicon dioxide were added to the reactor and stirred evenly. Then 0.75 g of hexadecyltrimethoxysilane was added and calcined at 145° C. for 2 h to obtain the first active silicon dioxide.
[0039] Preparation Example 2
[0040] The preparation steps of the second active silica are as follows:
[0041] 7.5 mL of 20 wt % sodium hydroxide solution and 10 g of silicon dioxide were added to the reactor, stirred evenly, and then 0.5 g of hexadecyltrimethoxysilane was added, and calcined at 145° C. for 2 h to obtain the second active silicon dioxide.
[0042] Preparation Example 3
[0043] The preparation steps of the third active silicon dioxide are as follows:
[0044] 7.5 mL of 20 wt % sodium hydroxide solution and 10 g of silicon dioxide were added to the reactor, stirred evenly, and then 1.1 g of hexadecyltrimethoxysilane was added, and calcined at 145° C. for 2 h to obtain the third active silicon dioxide.
[0045] Example 1
[0046] A alkali reducing agent with an antiseptic effect, the alkali reducing agent comprising the following raw materials in parts by weight: 2.5 parts of a first active silicon dioxide, 2.25 parts of a phosphonocarboxylic acid copolymer, 1.7 parts of cellulose ether, 1 part of ferrous sulfate, 1.25 parts of naphthalenesulfonic acid formaldehyde condensate sodium salt and 0.75 parts of ethylenediaminetetraacetic acid;
[0047] The preparation method of the alkali reducing agent with antiseptic effect in this embodiment comprises the following steps:
[0048] The first active silicon dioxide, phosphonocarboxylic acid copolymer, cellulose ether, ferrous sulfate, naphthalenesulfonic acid formaldehyde condensate sodium salt and ethylenediaminetetraacetic acid are sequentially mixed and stirred evenly to obtain an alkali reducing agent with an antiseptic effect.
[0049] Example 2
[0050] A alkali reducing agent with an antiseptic effect, the alkali reducing agent comprising the following raw materials in parts by weight: 2 parts of a first active silicon dioxide, 2 parts of a phosphonocarboxylic acid copolymer, 0.5 parts of a cellulose ether, 0.5 parts of ferrous sulfate, 1 part of a naphthalenesulfonic acid formaldehyde condensate sodium salt and 0.5 parts of ethylenediaminetetraacetic acid;
[0051] The preparation method of the alkali reducing agent with antiseptic effect in this embodiment comprises the following steps:
[0052] The first active silicon dioxide, phosphonocarboxylic acid copolymer, cellulose ether, ferrous sulfate, naphthalenesulfonic acid formaldehyde condensate sodium salt and ethylenediaminetetraacetic acid are sequentially mixed and stirred evenly to obtain an alkali reducing agent with an antiseptic effect.
[0053] Example 3
[0054] A alkali reducing agent with an antiseptic effect comprises the following raw materials in parts by weight: 3 parts of a first active silicon dioxide, 2.5 parts of a phosphonocarboxylic acid copolymer, 2.5 parts of cellulose ether, 1.5 parts of ferrous sulfate, 1.5 parts of naphthalenesulfonic acid formaldehyde condensate sodium salt and 1 part of ethylenediaminetetraacetic acid.
[0055] The preparation method of the alkali reducing agent with antiseptic effect in this embodiment comprises the following steps:
[0056] The first active silicon dioxide, phosphonocarboxylic acid copolymer, cellulose ether, ferrous sulfate, naphthalenesulfonic acid formaldehyde condensate sodium salt and ethylenediaminetetraacetic acid are sequentially mixed and stirred evenly to obtain an alkali reducing agent with an antiseptic effect.
[0057] Example 4
[0058] A alkali reducing agent with an antiseptic effect and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the first active silicon dioxide is replaced by an equal amount of the second active silicon dioxide.
[0059] Example 5
[0060] A alkali reducing agent with an antiseptic effect and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the first active silicon dioxide is replaced by an equal amount of a third active silicon dioxide.
[0061] Example 6
[0062] A alkali reducing agent with an antiseptic effect, the alkali reducing agent comprising the following raw materials in parts by weight: 2.5 parts of a first active silicon dioxide, 2.25 parts of a phosphonocarboxylic acid copolymer, 1.7 parts of cellulose ether, 1 part of ferrous sulfate, 1.25 parts of naphthalenesulfonic acid formaldehyde condensate sodium salt, 0.75 parts of ethylenediaminetetraacetic acid and 0.2 parts of octadecanoic acid;
[0063] The preparation method of the alkali reducing agent with antiseptic effect in this embodiment comprises the following steps:
[0064] The first active silicon dioxide, phosphonocarboxylic acid copolymer, cellulose ether, ferrous sulfate, naphthalenesulfonic acid formaldehyde condensate sodium salt, ethylenediaminetetraacetic acid and octadecanoic acid are sequentially mixed and stirred evenly to obtain an alkali reducing agent with an antiseptic effect.
[0065] Example 7
[0066] A alkali reducing agent with an antiseptic effect, the alkali reducing agent comprising the following raw materials in parts by weight: 2.5 parts of a first active silicon dioxide, 2.25 parts of a phosphonocarboxylic acid copolymer, 1.7 parts of cellulose ether, 1 part of ferrous sulfate, 1.25 parts of naphthalenesulfonic acid formaldehyde condensate sodium salt, 0.75 parts of ethylenediaminetetraacetic acid and 0.11 parts of octadecanoic acid;
[0067] The preparation method of the alkali reducing agent with antiseptic effect in this embodiment comprises the following steps:
[0068] The first active silicon dioxide, phosphonocarboxylic acid copolymer, cellulose ether, ferrous sulfate, naphthalenesulfonic acid formaldehyde condensate sodium salt, ethylenediaminetetraacetic acid and octadecanoic acid are sequentially mixed and stirred evenly to obtain an alkali reducing agent with an antiseptic effect.
[0069] Example 8
[0070] A alkali reducing agent with an antiseptic effect, the alkali reducing agent comprising the following raw materials in parts by weight: 2.5 parts of a first active silicon dioxide, 2.25 parts of a phosphonocarboxylic acid copolymer, 1.7 parts of cellulose ether, 1 part of ferrous sulfate, 1.25 parts of naphthalenesulfonic acid formaldehyde condensate sodium salt, 0.75 parts of ethylenediaminetetraacetic acid and 0.34 parts of octadecanoic acid;
[0071] The preparation method of the alkali reducing agent with antiseptic effect in this embodiment comprises the following steps:
[0072] The first active silicon dioxide, phosphonocarboxylic acid copolymer, cellulose ether, ferrous sulfate, naphthalenesulfonic acid formaldehyde condensate sodium salt, ethylenediaminetetraacetic acid and octadecanoic acid are sequentially mixed and stirred evenly to obtain an alkali reducing agent with an antiseptic effect.
[0073] Comparative Example 1
[0074] A alkali reducing agent with anti-corrosion effect and a preparation method thereof. The specific implementation method is the same as that of Example 6, except that the phosphonocarboxylic acid copolymer is replaced by an equal amount of a corrosion and scale inhibitor PO-600.
[0075] Comparative Example 2
[0076] A alkali reducing agent with an antiseptic effect and a preparation method thereof. The specific implementation method is the same as that of Example 6, except that an equal amount of silicon dioxide is used to replace the first active silicon dioxide.
[0077] Performance Test:
[0078] The alkali reducing agents prepared in the above examples and comparative examples were tested for the following properties, and the test results are shown in Table 1:
[0079] (1) Corrosion inhibition performance test: The rotating coupon corrosion test method was used. The test water used was the standard configuration water recommended by GB18175-2000. The test piece was A3 carbon steel with a size of 50 mm × 25 mm × 2 mm. The corrosion inhibition performance test was carried out as follows: Corrosion inhibition rate (%) = (X0-X1) / X0×100%, where: X0 (mm / a)-corrosion rate of the blank test piece without adding the alkali reducing agent; X1 (mm / a)-corrosion rate of the test piece with the alkali reducing agent added;
[0080] (2) Scale inhibition performance test: Static scale inhibition method - calcium carbonate deposition method, refer to GB / T16632-2008, scale inhibition rate = (ρ-ρ0) / (ρ1-ρ0)×100%, where: ρ - Ca after adding water treatment agent to the test solution and the scale inhibition test is completed 2+ Concentration, mg / mL; ρ0-Ca after the blank test solution scale inhibition test 2+ Concentration, mg / mL; ρ1-Ca in the test solution prepared before the scale inhibition test 2+ Concentration, mg / mL.
[0081] Table 1
[0082] project Corrosion inhibition rate / % Scale inhibition rate / % Example 1 96.7 95.8 Example 2 96.3 95.5 Example 3 96.5 94.8 Example 4 94.1 93.4 Example 5 93.9 94.1 Example 6 97.8 97.1 Example 7 97.5 96.6 Example 8 97.1 96.3 Comparative Example 1 92.1 93.0 Comparative Example 2 87.5 90.2
[0083] As can be seen from Table 1, the alkali reducing agent prepared in Examples 1 to 3 of the present invention is an environmentally friendly agent for boilers with excellent comprehensive performance, a reasonable and scientific formula, and synergistic effects of various components. While effectively reducing the alkalinity of boiler water, it also exerts an excellent corrosion and scale inhibition effect;
[0084] In Example 4 and Example 5, the preparation ratio of the active silicon dioxide is changed. Compared with Example 1, it can be shown that the active silicon dioxide preferably prepared in the present invention has good compatibility with the organic components in the alkali reducing agent. On the one hand, the active silicon dioxide is promoted to react with the inorganic base to form silicate; on the other hand, the generated silicate is used to adsorb and bind impurities such as iron oxide and manganese oxide to form insoluble precipitates, and the alkali reduction, corrosion prevention and scale inhibition effects are simultaneously achieved through boiler water discharge, effectively protecting the pipelines of the boiler water system;
[0085] Example 6 added octadecanoic acid at a specific mass ratio, while Examples 7 and 8 changed the mass ratio of octadecanoic acid to the corrosion and scale inhibitor. Compared with Example 1, both of them exerted a better synergistic scale inhibition effect, but the corrosion inhibition rate and scale inhibition rate were slightly lower than the specific mass ratio, indicating that the components of the alkali reducer system prepared specifically in the present invention exerted a better synergistic scale inhibition effect, which significantly improved the corrosion and scale inhibition effect.
[0086] In comparative example 1, the corrosion and scale inhibitor PO-600 is used to replace the phosphonocarboxylic acid copolymer in equal amounts, and the corrosion and scale inhibition effect of the system is not very significant. The possible reason is that the addition of octadecanoic acid increases the dispersion stability of the system and the solubility of other components, and all performances are improved; especially when the amount of corrosion and scale inhibitor added is reduced, the corrosion and scale inhibition effect does not show a significant decrease. The possible reason is that the surfactant promotes the dissociation of the -COOH group of the corrosion and scale inhibitor to a certain extent, that is, it plays a better synergistic scale inhibition effect, which means that the addition of the surfactant can reduce the amount of corrosion and scale inhibitor added and reduce the water treatment cost;
[0087] In Comparative Example 2, an equal amount of silicon dioxide is used to replace the first active silicon dioxide. The corrosion and scale inhibition effects of the alkali reducer system are affected, especially the corrosion inhibition rate decreases significantly. This may be due to the deterioration of its compatibility with the organic components in the alkali reducer, and its binding effect on impurities such as iron oxide and manganese oxide is hindered, making it difficult to effectively play the role of preventing pipeline corrosion.
[0088] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A alkali reducing agent with an antiseptic effect, characterized in that: The alkali reducing agent comprises the following raw materials in parts by weight: 2-3 parts of active silicon dioxide, 2-2.5 parts of corrosion and scale inhibitor, 0.8-2.5 parts of cellulose ether, 0.5-1.5 parts of ferrous sulfate, 1-1.5 parts of naphthalenesulfonic acid formaldehyde condensate sodium salt and 0.5-1 parts of ethylenediaminetetraacetic acid.
2. The alkali reducing agent with antiseptic effect according to claim 1, characterized in that: The preparation steps of the active silicon dioxide are as follows: Add 10-30 wt% of inorganic alkali solution and silicon dioxide into a reactor, stir evenly, then add a coupling agent, and calcine at 120-170° C. for 1-3 hours to obtain the active silicon dioxide.
3. The antiseptic alkali reducing agent according to claim 2, characterized in that: The mass ratio of the inorganic alkali solution to silicon dioxide is (0.5-1):
1.
4. The alkali reducing agent with antiseptic effect according to claim 2, characterized in that: The mass ratio of the coupling agent to silicon dioxide is (0.05-0.1):
1.
5. The alkali reducing agent with antiseptic effect according to claim 2, characterized in that: The particle size of the silicon dioxide is 20 to 100 meshes.
6. The alkali reducing agent with antiseptic effect according to claim 1, characterized in that: The corrosion and scale inhibitor is a phosphonocarboxylic acid copolymer with a number average molecular weight of 2000-4000.
7. The alkali reducing agent with antiseptic effect according to claim 1, characterized in that: The alkalinity reducing agent also adds octadecanoic acid.
8. The antiseptic alkali reducing agent according to claim 7, characterized in that: The mass ratio of the corrosion inhibitor and scale inhibitor to octadecanoic acid is 1:(0.06-0.13).
9. A method for preparing the antiseptic alkali reducing agent according to any one of claims 1 to 6, characterized in that: The following steps are involved: Active silicon dioxide, corrosion and scale inhibitor, cellulose ether, ferrous sulfate, sodium salt of naphthalenesulfonic acid formaldehyde condensate and ethylenediaminetetraacetic acid are sequentially mixed and stirred evenly to obtain the alkali reducing agent.
10. Use of the alkali reducing agent according to any one of claims 1 to 7 or the alkali reducing agent obtained by the preparation method according to claim 9 in a low-pressure steam boiler.
Citation Information
Patent Citations
Toilet deodorizing scale inhibitor
CN104629961A
High-effective composite corrosion and scale inhibitor being suitable for high-calcium and -alkali water and preparation method thereof
CN105130019A
Alkali inhibitor used for ordinary Portland cement
CN105503031A
corrosion and scale inhibitor
RU2014127411A