Colored glaze curtain wall and preparation method thereof
By using broken glass and specific temperature curve treatment, combined with reasonable raw material formulas and additives, the high cost and bubble problems of glazed curtain walls are solved, low-cost and high-quality glazed curtain wall production is achieved, and industrialization is promoted.
Patent Information
- Application Number
- CN202411242778.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The production cost of glass curtain walls is high and easy to produce bubbles, which affects the beauty and quality, resulting in the inability to form industrialization.
Broken glass is used as the main constituent material, and the temperature is increased and cooled by a specific temperature curve, combined with reasonable raw material formulas and additives, avoid the generation of bubbles and improve process stability, forming a beautiful and high-quality glazed curtain wall.
It reduces the production cost of glazed curtain walls, avoids bubble problems, improves the yield and aesthetics of products, and promotes the industrial production of glazed curtain walls.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glazed curtain walls, in particular to a glazed curtain wall and a preparation method thereof. Background Art
[0002] Colored glaze is a handicraft with Chinese national characteristics. Glass handicrafts use glass of various materials as raw materials. Through the conception and creation of artists, they fully express the characteristics of flowing colors and crystal clear quality. It has profound cultural connotations. Modern buildings are also trying to use colored glaze as curtain wall materials to enhance the beauty of the building.
[0003] However, the production cost of glazed curtain walls is high, and large bubbles are easily generated in the glazed curtain walls during the current production process, which affects the appearance and quality. At the same time, it is impossible to form flowing and colorful patterns in the glazed curtain walls, resulting in the glazed curtain walls being unable to be industrialized. Summary of the invention
[0004] The purpose of the present invention is to provide a glazed curtain wall and a preparation method thereof. The preparation method has low cost, is not prone to generate large bubbles, has a stable process, and the prepared glazed curtain wall has both beauty and quality.
[0005] The technical solution adopted by the present invention is: a method for preparing a glazed curtain wall, comprising the following steps: S1. Mix the raw materials of the glazed curtain wall mainly composed of broken glass in a mixer; the broken glass can be the defective products in the production process, which has a greater cost reduction compared with the normal chemical raw materials for preparing the glazed curtain wall; S2, putting the stirred glass curtain wall raw materials into the mold with uniform thickness, and sending the mold as a whole into the furnace; S3, heating according to the following temperature curve: The heating rate from room temperature to 600°C is 4 to 7°C / min; The heating rate from 600 to 1020°C is 3 to 5°C / min; Keep at 1020℃ for 30min; 1020~The heating rate of the highest temperature is 2~3℃ / min; The highest temperature is kept warm for 120 to 180 minutes; The highest temperature range is 1150~1250℃.
[0006] When this temperature rise curve is used for processing, the processed product is not prone to bubbles; S4. Cool down according to the following temperature curve: The cooling rate from the highest temperature to 900°C is 10-20°C / min; The cooling rate from 900 to 600°C is 0.5 to 1.5°C / min; The cooling rate from 600 to 400°C is 0.15 to 0.25°C / min; The cooling rate from 400 to 200°C is 0.2 to 0.25°C / min; The cooling rate from 200 to 90°C is 0.3 to 0.4°C / min; When the temperature is 90°C, the blank is placed at room temperature and cooled for 4 to 6 hours to obtain a glazed curtain wall blank; When this cooling curve is used for processing, the stress generated by the product annealing process can be reduced, ensuring the product yield; S5, after the glazed curtain wall blank is unloaded, it is polished to obtain a glazed curtain wall finished product with uniform thickness; As a preferred solution, the broken glass is broken tempered glass. When broken tempered glass is used, the effect of the produced glazed curtain wall is the best.
[0007] As a preferred solution, the glazed curtain wall raw material also includes additives, which are mixed according to the chemical composition of the cullet so that the components of the glazed curtain wall raw material are maintained within the following ranges by mass: SiO2 70~85 parts Al2O3 2~6 parts CaO 8~15 parts MgO 2~6 parts B2O3 6 to 13 parts.
[0008] According to the chemical composition of the cullet, additives are mixed to make the raw materials of the glazed curtain wall include the following components by mass: Na2O / K2O 0~9 parts BaO 0~2 parts PbO 0~5 parts Li2O 0 to 3 parts.
[0009] in: Na2O / K2O: Reduce glass viscosity; BaO: helps crystallization and improves the structural strength of the glazed curtain wall; PbO: improves the density and refractive index of the glass curtain wall; Li2O: Its introduction can reduce the expansion coefficient of the glass curtain wall material and improve thermal stability.
[0010] As a preferred solution, the amount of broken glass used is not less than 60% of the total weight of the raw materials of the glazed curtain wall, ensuring low processing costs.
[0011] As a preferred embodiment, the additive is one or more of boric acid, high-lead frit, spodumene and soda ash.
[0012] As a preferred embodiment, the additive further comprises 0 to 2 parts of a colored metal oxide; after adding the colored metal oxide, the finished product has colored textures; The colored metal oxide is an oxide of Fe, Cu, Co, Mn, Ni or Cr.
[0013] As a preferred solution, the glass curtain wall raw materials other than the colored metal oxide are uniformly mixed in step S1, and the colored metal oxide is unevenly mixed in the glass curtain wall raw materials in step S2. The uneven mixing can obtain more natural colored glass textures.
[0014] As a preferred solution, the particle size of the broken glass is 2 to 5 cm, and the thickness of the glazed curtain wall raw material in the mold is about twice the thickness of the finished glazed curtain wall.
[0015] A glazed curtain wall is manufactured by using the above-mentioned glazed curtain wall preparation method.
[0016] Compared with the prior art, the present invention has the following beneficial effects: 1. In the preparation method of the glazed curtain wall, the raw material is the broken glass formed by failed or defective products in the glass production process. The broken glass only costs 300 to 400 yuan per ton, which is a significant reduction in cost compared with the previous one; 2. In the preparation method of the glazed curtain wall, the temperature is raised and lowered through a reasonable temperature curve to avoid large bubbles in the product and reduce the stress generated by the product annealing process, which can ensure the success rate of the finished glazed curtain wall and is conducive to the industrialization of the processing of the glazed curtain wall; 3. In the preparation method of the glazed curtain wall, the formula of the raw materials of the glazed curtain wall is reasonably configured, and the temperature curve is matched to improve the stability of the process; 4. In the preparation method of the colored glaze curtain wall, colored metal oxides are added, and natural colored lines of colored glaze can be produced through the natural flow of the melt during the firing process; 5. The produced glazed curtain wall has a transparent texture, with micron-sized bubbles evenly distributed inside the glazed glass, and no large bubbles are generated, which combines beauty and quality. DETAILED DESCRIPTION
[0017] The present invention is described in detail below by way of exemplary embodiments. However, it should be understood that, without further description, elements, structures and features in one embodiment may also be beneficially combined in other embodiments.
[0018] It should be noted that: unless otherwise defined, the technical terms or scientific terms used in this document shall have the usual meanings understood by people with ordinary skills in the field to which the invention belongs. The words "one", "an" or "the" and the like used in the patent application specification and claims of the present invention do not express quantity restrictions, but indicate the existence of at least one; the words "first", "second" and "third" used in this document shall not be regarded as restrictions on the order of components, but are only used to distinguish different components; words such as "include" or "comprise" and the like indicate that the elements or objects appearing before "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, but do not exclude other elements or objects with the same function.
[0019] The present invention provides a method for preparing a glazed curtain wall, comprising the following steps: S1. Select or process broken glass with a particle size of 2 to 5 cm, and mix the raw materials of the glazed curtain wall mainly composed of broken glass or broken tempered glass in a mixer; the amount of broken glass should preferably not be less than 60% of the total weight of the raw materials of the glazed curtain wall; Additives (one or more of boric acid, high-lead frit, spodumene and soda ash) are mixed according to the chemical composition of the cullet to keep the composition of the glass curtain wall raw materials (cullet and additives) within the following range by mass: SiO2 70-85 parts, Al2O3 2-6 parts, CaO 8-15 parts, MgO 2-6 parts, B2O3 6-13 parts, Na2O / K2O 0-9 parts, BaO 0-2 parts, PbO 0-5 parts, Li2O 0-3 parts; S2, putting the stirred glass curtain wall raw materials into the mold with uniform thickness, and sending the mold as a whole into the furnace; S3, heating according to the following temperature curve: The heating rate from room temperature to 600℃ is 4~7℃ / min; this section is the early preheating stage. Since the glazed curtain wall is thick, the thickness of the glass material in the mold is 12~20cm, and sufficient time is required to preheat the material inside the mold; The heating rate from 600 to 1020°C is 3 to 5°C / min. This section is the heating section. When the heating rate is within this range, the glass material can be heated evenly inside and outside, and the temperature difference between the inside and outside is small, which is conducive to the synchronous melting of the inner and outer glass materials, and avoids the surface glass material melting too fast and the internal glass material melting too slowly, which causes the glass material to be stuck. Keep warm at 1020℃ for 30min. This section is the heat preservation section. The reason for keeping warm at this temperature is that a large amount of liquid phase has begun to appear in the glass material at this temperature. In order to slow down the melting process, the gaps between the glass materials are slowly filled with the glass material melt to avoid the internal gas from being unable to be discharged due to premature closure of the surface. The heating rate from 1020 to the highest temperature is 2-3℃ / min. The heating rate in this section is slower than before in order to allow the glass material to have sufficient exhaust process. The highest temperature insulation time is 120 to 180 minutes; the highest temperature insulation is to allow the entire glazed curtain wall to complete the densification process and make the product completely homogenized inside and outside; Among them: the highest temperature range is 1150~1250℃; S4. Cool down according to the following temperature curve: The cooling rate from the highest temperature to 900℃ is 10~20℃ / min; this section is the rapid cooling section, and the entire product is still in a molten state, so the rapid cooling will not cause stress inside the product; The cooling rate from 900 to 600℃ is 0.5 to 1.5℃ / min. This section is the slow cooling stage after the rapid cooling stage. Since a large amount of heat is still stored inside the glazed curtain wall, it can be cooled at a faster rate. However, cold air cannot be blown directly in this section. The cooling rate from 600 to 400°C is 0.15 to 0.25°C / min. The cooling rate in this temperature range is significantly slower because there is a crystal transformation process of quartz in this section. In order to avoid stress inside the glass curtain wall and cause cracking, the cooling rate is controlled within this range. The cooling rate of 400-200℃ is 0.2-0.25℃ / min. The cooling rate of this section is higher than that of the previous section, which can achieve rapid cooling of the product. However, the cooling rate should not be too fast, which will also cause a large temperature difference between the inside and outside of the product and cause stress cracking. Therefore, 0.2-0.25℃ / min is appropriate. The cooling rate of 200-90℃ is 0.3-0.4℃ / min; below 200℃, the cooling rate can be further increased, and the glass curtain wall will not burst in this section. However, due to the large heat storage of the glass curtain wall, it is not easy to discharge, so even if the cooling rate is faster, the internal heat cannot be discharged. Therefore, the cooling rate of 0.3-0.4℃ / min is the optimal cooling rate. When the temperature is 90°C, the blank is placed at room temperature and cooled for 4 to 6 hours to obtain a glazed curtain wall blank; S5. After the glazed curtain wall blank is unloaded, it is polished to obtain a glazed curtain wall finished product with uniform thickness.
[0020] The additives also include colored metal oxides, which are oxides of Fe, Cu, Co, Mn, Ni or Cr. Different from the above processing method, when coloring is required, the glazed curtain wall raw materials except the colored metal oxides are uniformly mixed in step S1, and in step S2, 0 to 2 parts of the colored metal oxides are unevenly mixed in the glazed curtain wall raw materials, and finally a glazed curtain wall finished product with colorful cloud-like flow patterns is obtained.
[0021] A glazed curtain wall is manufactured by adopting the glazed curtain wall preparation method.
[0022] In order to describe the present invention more clearly, the following is further described in detail with reference to the embodiments: Embodiment 1: (1) Weigh 200 kg of broken glass, 50 kg of borax, 30 kg of high-lead frit and 20 kg of soda ash according to the weight ratio and put them into a drum cement mixer to mix.
[0023] (2) Prepare the mold and apply a layer of release agent on the inside of the mold.
[0024] (3) Place the mixed material in the mold with a thickness of 14 cm.
[0025] (4) Put it into the furnace and heat it up according to the following temperature curve: a. The heating rate from room temperature to 600°C is 7°C / min.
[0026] b. The heating rate from 600 to 1020°C is 5°C / min.
[0027] c. Keep at 1020℃ for 30min.
[0028] d. The heating rate from 1020 to 1180°C is 3°C / min.
[0029] e. Keep at 1180℃ for 120min.
[0030] (5) Cool down according to the following temperature curve: A. The cooling rate from 1180 to 900°C is 20°C / min.
[0031] B. The cooling rate from 900 to 600°C is 1.5°C / min.
[0032] C. The cooling rate from 600 to 400°C is 0.25°C / min.
[0033] D. The cooling rate from 400 to 200°C is 0.25°C / min.
[0034] E. The cooling rate from 200 to 90°C is 0.4°C / min.
[0035] F. After cooling at 90℃ for 4 hours at room temperature, unload the glazed curtain wall blank product.
[0036] (6) The glazed curtain wall blank is polished and finished to obtain a glazed curtain wall product with a thickness of 6 cm.
[0037] Embodiment 2: (1) Weigh 400 kg of broken glass, 120 kg of borax, 80 kg of high-lead frit, 40 kg of spodumene, and 20 kg of soda ash according to the weight ratio and put them into a drum cement mixer for mixing.
[0038] (2) Prepare the mold and apply a layer of release agent on the inside of the mold.
[0039] (3) The mixed material is placed in a mold with a thickness of 20 cm. During the material application process, 500 g of cobalt oxide (coloring metal oxide) is unevenly spread into the material.
[0040] (4) Put it into the furnace and heat it up according to the following temperature curve: a. The heating rate from room temperature to 600°C is 4°C / min.
[0041] b. The heating rate from 600 to 1020°C is 3°C / min.
[0042] c. Keep at 1020℃ for 30min.
[0043] d. The heating rate from 1020 to 1180°C is 2°C / min.
[0044] e. Keep at 1230℃ for 180min.
[0045] (5) Cool down according to the following temperature curve: A. The cooling rate from 1230 to 900°C is 10°C / min.
[0046] B. The cooling rate from 900 to 600°C is 1°C / min.
[0047] C. The cooling rate from 600 to 400°C is 0.15°C / min.
[0048] D. The cooling rate from 400 to 200°C is 0.2°C / min.
[0049] E. The cooling rate from 200 to 90°C is 0.3°C / min.
[0050] F. After cooling at 90℃ for 6 hours at room temperature, unload the glazed curtain wall blank product.
[0051] (6) The glazed curtain wall blank is polished and polished, and a glazed curtain wall product with a thickness of 10 cm is obtained after the processing. There will be blue cloud-like flow patterns in the glazed curtain wall.
[0052] Embodiment three: A building glazed curtain wall and a preparation method thereof, comprising the following steps: (1) Weigh 460 kg of broken glass, 60 kg of borax, 20 kg of high-lead frit and 40 kg of soda ash according to the weight ratio and put them into a drum cement mixer to mix.
[0053] (2) Prepare the mold and apply a layer of release agent on the inside of the mold.
[0054] (3) Place the mixed material in the mold with a thickness of 20 cm.
[0055] (4) Put it into the furnace and heat it up according to the following temperature curve: a. The heating rate from room temperature to 600°C is 4°C / min.
[0056] b. The heating rate from 600 to 1020°C is 3°C / min.
[0057] c. Keep at 1020℃ for 30min.
[0058] d. The heating rate from 1020 to 1250°C is 2°C / min.
[0059] e. Keep at 1250℃ for 120min.
[0060] (5) Cool down according to the following temperature curve: A. The cooling rate from 1180℃ to 900℃ is 15℃ / min.
[0061] B. The cooling rate from 900 to 600°C is 1°C / min.
[0062] C. The cooling rate from 600 to 400°C is 0.15°C / min.
[0063] D. The cooling rate from 400℃ to 200℃ is 0.2℃ / min.
[0064] E. The cooling rate from 200℃ to 90℃ is 0.3℃ / min.
[0065] F. After cooling at 90℃ for 4 hours at room temperature, unload the glazed curtain wall blank product.
[0066] (6) The glazed curtain wall blank is polished and finished to obtain a glazed curtain wall product with a thickness of 10 cm.
[0067] The parts not described in detail in this embodiment are prior art.
[0068] It should be noted that although the present invention is described by the above embodiments, the present invention may also have other various embodiments. Without departing from the spirit and scope of the present invention, it is obvious that those skilled in the art may make various corresponding changes and deformations to the present invention, but these changes and deformations should all fall within the scope of protection of the appended claims of the present invention and their equivalents.
Claims
1. A method for preparing a glazed curtain wall, characterized in that: The following steps are involved: S1. Mixing the raw materials of the glazed curtain wall mainly composed of broken glass in a mixer; S2, putting the stirred glass curtain wall raw materials into the mold with uniform thickness, and sending the mold as a whole into the furnace; S3, heating according to the following temperature curve: The heating rate from room temperature to 600°C is 4 to 7°C / min; The heating rate from 600 to 1020°C is 3 to 5°C / min; Keep at 1020℃ for 30min; 1020~The heating rate of the highest temperature is 2~3℃ / min; The highest temperature is kept warm for 120 to 180 minutes; Among them: the highest temperature range is 1150~1250℃; S4. Cool down according to the following temperature curve: The cooling rate from the highest temperature to 900°C is 10-20°C / min; The cooling rate from 900 to 600°C is 0.5 to 1.5°C / min; The cooling rate from 600 to 400°C is 0.15 to 0.25°C / min; The cooling rate from 400 to 200°C is 0.2 to 0.25°C / min; The cooling rate from 200 to 90°C is 0.3 to 0.4°C / min; When the temperature is 90°C, the product is placed at room temperature and cooled for 4 to 6 hours to obtain a glazed curtain wall blank; S5. After the glazed curtain wall blank is unloaded, it is polished to obtain a glazed curtain wall finished product with uniform thickness.
2. The method for preparing a glazed curtain wall according to claim 1, characterized in that: The broken glass is broken tempered glass.
3. The method for preparing a glazed curtain wall according to claim 1, characterized in that: The raw materials of the glazed curtain wall also include additives, which are mixed according to the chemical composition of the cullet so that the components of the raw materials of the glazed curtain wall are kept within the following ranges by mass: SiO270~85 parts Al2O32~6 parts CaO 8~15 parts MgO 2~6 parts B2O36~13 parts.
4. The method for preparing a glazed curtain wall according to claim 3, characterized in that: According to the chemical composition of the cullet, additives are mixed to make the raw materials of the glazed curtain wall include the following components by mass: Na2O / K2O 0~9 parts BaO 0~2 parts PbO 0~5 parts Li2O 0 to 3 parts.
5. The method for preparing a glazed curtain wall according to claim 1, characterized in that: The amount of broken glass used shall not be less than 60% of the total weight of the raw materials of the glazed curtain wall.
6. A method for preparing a glazed curtain wall according to claim 3 or 4, characterized in that: The additive is one or more of boric acid, high-lead frit, spodumene and soda ash.
7. A method for preparing a glazed curtain wall according to claim 3 or 4, characterized in that: The additives also include 0 to 2 parts by mass of a coloring metal oxide; The colored metal oxide is an oxide of Fe, Cu, Co, Mn, Ni or Cr.
8. The method for preparing a glazed curtain wall according to claim 7, characterized in that: The glazed curtain wall raw materials except the colored metal oxide are uniformly mixed in step S1, and the colored metal oxide is non-uniformly mixed in the glazed curtain wall raw materials in step S2.
9. The method for preparing a glazed curtain wall according to claim 1, characterized in that: The particle size of the broken glass is 2 to 5 cm.
10. A glazed curtain wall, characterized in that: The glazed curtain wall is manufactured by using the preparation method of a glazed curtain wall according to any one of claims 1 to 9.