Method for preparing optical fiber preform through in-tube method
By adjusting the flow rate of the reactive gas in different sections within the quartz tube, the problem of substandard results at both ends of the core rod was solved, achieving efficient preparation of optical fiber preforms and improved material utilization.
Patent Information
- Application Number
- CN202410957743.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional mandrel manufacturing methods result in the mandrel ends being unable to meet the wire drawing requirements of subsequent production, leading to a waste of production materials.
By dividing the chemical deposition process within the quartz tube into multiple sub-regions and adjusting the reaction gas flow rate according to the location of the excitation source and the gas inlet control structure, the reaction gas flow rate within each sub-region is ensured to change continuously, thereby improving the axial consistency of the mandrel and increasing the effective mandrel length.
This improved the precision and effective length of optical fiber preforms, reduced waste of production materials, and increased the yield of qualified optical fibers.
Smart Images

Figure CN118908560A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical fiber production, and in particular to a method for preparing an optical fiber preform rod using an in-tube method. Background Art
[0002] When preparing the core rod by the vapor deposition process, the refractive index distribution of the optical fiber is adjusted by adding dopants (such as Ge, P, F, B, Al, Ti, Zr, etc.) to SiO2. The deposited quartz glass tube is melted and condensed in a high-temperature furnace to prepare a solid core rod. Then, the core rod is corroded, cleaned, and dried, and then combined with the matching sleeve to form an optical fiber preform rod, which is drawn into an optical fiber by a drawing device.
[0003] The performance of optical fiber mainly depends on the parameters of optical fiber preform. The fluctuation of axial parameters of optical fiber preform directly affects the consistency of optical fiber performance. Therefore, the uniformity of axial parameters of optical fiber preform must be improved. When preparing the core rod by the in-tube method, the high-purity reactants undergo the above-mentioned chemical reaction and vapor deposition in the quartz glass tube. The mixed gas moves from the feed end to the discharge end in the tube. There are differences in the components, temperature, pressure, density, energy, etc. at each point in the axial distribution in the tube, which makes the cross-sectional parameters and structural strength of the core rod have certain deviations along its axial direction. This deviation is particularly obvious at the two ends of the core rod, which makes it difficult for the rod body at the two ends of the core rod to meet the drawing requirements of subsequent pipeline production. Therefore, the unqualified rod lengths at the two ends are generally removed, and the optical fiber is drawn with the effective rod length in the middle. This production method will undoubtedly cause waste of production materials. Summary of the invention
[0004] The main purpose of the present invention is to propose a method for preparing an optical fiber preform rod by an in-tube method, aiming to solve the problem that the traditional core rod preparation method cannot effectively increase the effective rod length of the core rod and easily leads to waste of production materials.
[0005] To achieve the above-mentioned purpose, the present invention provides a method for preparing an optical fiber preform rod by the in-tube method, comprising a preparation device, wherein the preparation device comprises a rotating mounting structure, a quartz tube, an excitation source and an air intake control structure, wherein the rotating mounting structure is used to fix the quartz tube and drive the quartz tube to rotate around its axis, wherein the air intake control structure is arranged at the air intake end of the quartz tube and is used to control the flow rate of the reaction gas at the air intake end of the quartz tube, wherein the excitation source has a movement stroke along the axis direction of the quartz tube and is used to promote the reaction gas to produce chemical deposition in the quartz tube, and wherein the method for preparing an optical fiber preform rod by the in-tube method comprises the following preparation processes:
[0006] Under the preset deposition conditions, the quartz tube is mounted on the rotating mounting structure, the excitation source is controlled to reciprocate along the axial direction of the quartz tube, each of the reaction gases is introduced into the quartz tube through the gas inlet control structure, and the reaction gases are chemically deposited in the quartz tube by the excitation source to form a preformed rod body; m sub-areas with m+1 axial points are divided along the axial direction of the preformed rod, and the flow opening of the gas inlet control structure is calibrated according to the cross-sectional parameters and bending strength parameters at each of the axial points to adjust the flow of each of the reaction gases to continuously change in each of the sub-areas
[0007] In one embodiment, the plurality of sub-regions are divided according to the cross-sectional parameters and the bending strength of the preform body, and the cross-sectional parameters in each sub-region gradually increase or decrease or remain substantially unchanged.
[0008] In one embodiment, the plurality of sub-regions include a first sub-region at the feed end of the quartz tube and a tail terminal region at the discharge end of the quartz tube, the first sub-region and the end corresponding to the tail terminal region are the gradient starting point and the gradient end point, respectively, and the first sub-region and the end separated from the tail terminal region are the first inflection point and the second inflection point, respectively;
[0009] The excitation source moves between the first inflection point and the second inflection point, and the total length of the preformed rod is L total , the L total is the distance between the first inflection point and the second inflection point; and / or,
[0010] The spacing between the plurality of axial points is L b , the L b ≤20mm.
[0011] In one embodiment, the reaction gas includes SiCl4 and O2;
[0012] In the first sub-zone, the reaction gas gradually increases from the gradual change starting point to the first inflection point; and\or,
[0013] In the tail terminal region, the reaction gas gradually decreases from the second inflection point to the gradual end point.
[0014] In one embodiment, in the first sub-area, the reaction gas gradually increases from the gradual change starting point to the first inflection point, and the increase rate of the reaction gas is 1% to 20%; and\or,
[0015] Each of the reaction gases includes at least one of SiCl4, O2, GeCl4, POCl3, C2F6 and BCl3.
[0016] In one embodiment, the reaction gas includes GeCl4 or POCl3;
[0017] In the first sub-zone, the reaction gas gradually decreases from the gradual change starting point to the first inflection point; and\or,
[0018] In the tail terminal region, the reaction gas gradually increases when moving from the second inflection point to the gradual end point.
[0019] In one embodiment, in the first sub-area, the reaction gas gradually decreases from the gradual change starting point to the first inflection point, and the reduction range of the reaction gas is 10% to 100%; and / or,
[0020] The distance from the gradual change starting point to the first inflection point is 20 mm to 200 mm, and the distance from the second inflection point to the gradual change end point is 20 mm to 190 mm.
[0021] In one embodiment, the reaction gas includes C2F6 or BCl3;
[0022] In the first sub-zone, the reaction gas gradually increases from the gradual change starting point to the first inflection point; and\or,
[0023] In the tail terminal region, the reaction gas gradually increases from the gradual end point to the second inflection point.
[0024] In one embodiment, in the first sub-area, the reaction gas gradually increases from the gradual change starting point to the first inflection point, and the increase rate of the reaction gas is 2% to 50%; and / or,
[0025] In the tail terminal region, the reaction gas gradually increases from the gradual end point to the second inflection point, and the increase rate of the reaction gas is 2% to 50%.
[0026] In one embodiment, the L total ≥500mm, the length of the first sub-area and the tail terminal area are both L, 0.03L total ≤L≤0.05L total ; and\or,
[0027] Among the plurality of sub-areas, at least one sub-area in which the reaction gas flow rate remains constant, and the length of the sub-area is set to L m , L m ≥ 0.2 L total .
[0028] The technical solution of the present invention can improve the axial consistency of the core rod by dividing the entire core layer deposition area into m areas and controlling the intake flow rate of the reaction gas through the intake control structure according to the position of the excitation source, thereby improving the preparation accuracy and effective rod length of the core layer of the gradient refractive index optical fiber preform rod, and increasing the output ratio of qualified optical fibers. In addition, in this solution, reasonable axial spacing is used to achieve partition adjustment and reasonable transition between partitions, avoiding frequent fluctuations in parameters, so that the deposition process is adjustable and stable. The method of the present invention is simple and effective, low in cost, and has strong feasibility and operability. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0030] Figure 1 A schematic diagram of a portion of the structure of a preparation device in the method for preparing an optical fiber preform using the in-tube method provided by the present invention;
[0031] Figure 2 for Figure 1 Flow chart of the method for preparing optical fiber preform rod by the inner tube method;
[0032] Figure 3 for Figure 1 Axial refractive index deviation distribution diagram of the embodiment and the comparative example when the reaction gas of the method for preparing the optical fiber preform rod in the middle tube method is GeCl4 or POCl3;
[0033] Figure 4 for Figure 1 Axial refractive index deviation distribution diagram of the embodiment and the comparative example of the method for preparing optical fiber preform rod by the inner tube method with the reaction gas being C2F6 or BCl3;
[0034] Figure 5 for Figure 1 The core diameter deviation distribution diagram of the embodiment and the comparative example of the method for preparing an optical fiber preform rod by the inner-tube method with the reaction gases being SiCl4 and O2.
[0035] Description of Figure Numbers:
[0036] 100. Preparation equipment; 1. Rotating mounting structure; 11. Rotating chuck device at the feeding end; 12. Rotating chuck device at the discharging end; 2. Quartz tube; 3. Air intake control structure; 31. First control valve; 32. Second control valve; 33. Flow controller; 4. Excitation source; 5. Insulating furnace; 6. Extension tube.
[0037] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0040] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if "and / or" or "and / or" appears in the full text, its meaning includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0041] When preparing the core rod by the vapor deposition process, the refractive index distribution of the optical fiber is adjusted by adding dopants (such as Ge, P, F, B, Al, Ti, Zr, etc.) to SiO2. The deposited quartz glass tube is melted and condensed in a high-temperature furnace to prepare a solid core rod. Then, the core rod is corroded, cleaned, and dried, and then combined with the matching sleeve to form an optical fiber preform rod, which is drawn into an optical fiber by a drawing device.
[0042] The performance of optical fiber mainly depends on the parameters of optical fiber preform. The fluctuation of axial parameters of optical fiber preform directly affects the consistency of optical fiber performance. Therefore, the uniformity of axial parameters of optical fiber preform must be improved. When preparing the core rod by the in-tube method, the high-purity reactants undergo the above-mentioned chemical reaction and vapor deposition in the quartz glass tube. The mixed gas moves from the feed end to the discharge end in the tube. There are differences in the components, temperature, pressure, density, energy, etc. at each point in the axial distribution in the tube, which makes the cross-sectional parameters and structural strength of the core rod have certain deviations along its axial direction. This deviation is particularly obvious at the two ends of the core rod, which makes it difficult for the rod body at the two ends of the core rod to meet the drawing requirements of subsequent pipeline production. Therefore, the unqualified rod lengths at the two ends are generally removed, and the optical fiber is drawn with the effective rod length in the middle. This production method will undoubtedly cause waste of production materials.
[0043] The invention provides a method for preparing an optical fiber preform rod by an in-tube method.
[0044] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0045] In the examples of the present invention, "first", "second", etc. are used to distinguish different objects, and are not necessarily used to describe a specific order or sequence.
[0046] To facilitate the introduction of the present invention, some terms are defined:
[0047] Flow meter (Mass Flow Controller, MFC): Mass flow controller, a gas flow stabilizing device that provides accurate reactant (such as GeCl4, C2F6, etc.) flow automatic control for core rod preparation.
[0048] Profile parameters: The profile refractive index of the optical fiber preform can be divided into multiple layers. The radius of each layer is the distance from the outer edge to the axis. The relative refractive index of each layer is the refractive index relative to the cladding, which is usually also the refractive index relative to pure silica. The geometric parameters of the profile include the diameter, roundness, concentricity, etc. of each layer, and the optical parameters include the relative refractive index and distribution index.
[0049] The core refractive index profile of the graded-index optical fiber needs to be designed to have a refractive index distribution that continuously and gradually decreases from the center to the edge of the core, which is usually called the "α profile". That is, the refractive index distribution satisfies the following power exponential function:
[0050]
[0051] Where n1: represents the refractive index of the optical fiber axis;
[0052] r: indicates the distance from the optical fiber axis;
[0053] a: represents the fiber core radius;
[0054] α: represents the distribution index;
[0055] Δ0: represents the refractive index of the core center relative to the cladding.
[0056] Relative refractive index, i.e. △i:
[0057]
[0058] Among them, n i : represents the refractive index at position i from the core center;
[0059] n0: represents the minimum refractive index of the optical fiber core, which is usually also the refractive index of the optical fiber cladding.
[0060] Core rod: a preform containing a core layer and part of the cladding. The total length of the core rod is the distance between the inflection points at both ends of the reciprocating motion, and the effective rod length is the length in which each section parameter meets the requirements of the production control range.
[0061] Mother rod: A reference core rod used to test the axial distribution of profile parameters, whose length is the effective rod length of the core rod.
[0062] See also Figures 1 to 5 In one embodiment of the present invention, the method for preparing the optical fiber preform rod in the tube method is as follows: Figure 1 The present invention is a schematic diagram of a preparation device 100 and a reactant supply, wherein a rotating mounting structure 1 comprises a rotating chuck device 11 at a feed end and a rotating chuck device 12 at a discharge end, which are used to fix the two ends of a quartz tube 2 respectively, and at the same time, the connecting driving structure can drive the quartz tube 2 to rotate around its axis direction to promote a uniform reaction of the gas in the tube, and each reaction gas controls the intake flow rate through an intake control structure 3 (comprising a first control valve 31, a second control valve 32 and a flow controller 33). After each reaction gas is introduced into the interior of the quartz tube 2, it is reciprocated along the axis direction of the quartz tube 2 through an excitation source 4, thereby promoting the reaction gas to produce chemical deposition on the inner wall of the quartz tube 2, and finally completing the preparation of the optical fiber core rod. In this embodiment, as shown in FIG. Figure 1As shown, the excitation source 4 adopts a high-frequency resonant cavity, and the glass deposition layer is generated on the inner wall of the high-purity quartz glass tube by reaction in the high-frequency resonant cavity that reciprocates at high speed. The reaction tail gas is extracted from the discharge end extension tube 6 and the discharge end rotating chuck device 12. The core rod after deposition is prepared into an optical fiber preform after melting and shrinking. The MCVD production equipment replaces the high-frequency resonant cavity in the figure with a flame blowtorch, and does not require a heat preservation furnace 5. Under certain specific deposition conditions, for example, the rotation speed of the quartz tube 2, the external temperature, the movement speed of the excitation source 4, and the working parameters are within a certain control range, the quartz tube 2 is installed on the rotating installation structure 1, the excitation source 4 is controlled to reciprocate along the axis direction of the quartz tube 2, and each of the reaction gases is introduced into the quartz tube 2 through the air intake control structure 3. In this process, the air intake control structure 3 can control the flow rate of each of the reaction gases, and the excitation source 4 is used to cause the reaction gas to produce chemical deposition in the quartz tube 2 to form a preform.
[0063] Considering that, in the actual production process, the axial distribution of the parameters of the core rod is affected by high-frequency equipment, motion system, high-temperature distribution, etc., there is a certain axial volatility. Since the excitation source 4 moves back and forth, there are acceleration and deceleration processes and movement speed fluctuations at both ends of the quartz tube 2, which will affect the uniform distribution of the axial temperature of the quartz tube 2 in the insulation furnace 5. Therefore, during the heating process of the reaction gas at the feed end of the quartz tube 2, the parameters of the deposited core rod preform near its feed end (IS) deviate from the ideal state and fluctuate violently. On the other hand, the air flow fluctuations caused by the exhaust at the discharge end of the quartz tube 2 and the gradual accumulation of dust in the pipe of the quartz tube 2 during the deposition process make the core rod parameter fluctuations in the area of the preform near the discharge end (OS) of the quartz tube 2 more significant.
[0064] Due to the uneven deposition, the two ends of the deposited rod are prone to the problem of geometric dimensions deviating from the center value, and the length of the two ends accounts for more than 5% of the total length of the rod. In order to increase the effective rod length, a common method is to appropriately extend the time of the excitation source 4 at the two ends of the reversing acceleration and deceleration process, but the reaction area of the reaction gas excited by the excitation source 4 has a certain length. If the residence time is too long, the geometric dimensions of the uniform area adjacent to the uneven areas at the two ends will be too large, and the effect of the above method is limited.
[0065] Based on the above actual situation, in order to increase the effective rod length of the prepared core rod and shorten the non-compliant length of the two ends of the rod body, in this embodiment, the air intake control structure 3 realizes the supply control of the reaction gas flow rate mainly according to the different positions of the excitation source 4 along the axial direction of the quartz tube 2, so that the cross-sectional parameters and mechanical properties of the areas at both ends of the rod body are as consistent as possible with the effective rod length area in the middle, and the effective rod length is increased as much as possible. Among them, after the preparation of the preform rod body (mother rod) is completed, firstly, m sub-areas with m+1 axial points are divided along the axial direction of the preform rod, and the cross-sectional parameters and bending strength parameters of each axial point are analyzed, and then the air intake flow of the air intake control structure 3 is corrected according to the analysis results, and the mapping correspondence between the position of the excitation source 4 and the working parameters of the air intake control structure 3 when the excitation source 4 is located at different axial points is obtained. That is, the flow opening of the intake control structure 3 is calibrated according to the cross-sectional parameters and bending strength parameters at each axial point to adjust the flow of each reaction gas to continuously change in each sub-area. After the flow opening of the intake control structure 3 is calibrated, the flow of different reaction gases is continuously controlled to reduce the differences in cross-sectional parameters and mechanical properties between the two end areas of the rod body and the middle effective rod length.
[0066] Among them, the multiple sub-areas are divided according to the profile parameters and bending strength of the preform rod body, and the profile parameters are used as the main basis for division. After analyzing the profile parameters of the multiple axial points, a corresponding profile parameter change curve can be generated. Generally, the partitions are performed at the inflection points of the change curve, and the profile parameters in each sub-area gradually increase or decrease or remain basically unchanged.
[0067] During the test, the entire mother rod is tested using a profile test device, and the test interval between the two axial points is ≤20mm, preferably ≤10mm, so that the distribution of the core rod parameters along the axial direction can be obtained. In order to ensure the accuracy of the data at this time, the test data can also be corrected with the optical fiber profile parameters after the test preform (mother rod) is drawn. The position of the optical fiber and the total length of the mother rod drawn can be converted into the axial position of the core rod corresponding to the profile parameters as auxiliary data. If the total length of the mother rod drawn is 200km, the test optical fiber is at the 100km, that is, the measured profile parameters are located at 50% of the axial length of the mother rod. According to the profile parameters after the mother rod is measured, the axial position of the core rod in the equipment can be divided into multiple regions according to the change of its parameters. The profile parameters can be the relative refractive index and diameter of each layer. If it is a gradient refractive index, it also includes its distribution index α. In this scheme, the main purpose is to improve the consistency of parameters between the two end regions of the preform rod body (mother rod) and the middle effective rod body. Therefore, in this embodiment, the first sub-region located at the feed end of the quartz tube 2 and the tail terminal region located at the discharge end of the quartz tube 2 are mainly targeted. The region between the ends of the first sub-region and the tail terminal region is the effective rod length region. The two ends of the effective rod length correspond to the end points of the first sub-region and the tail terminal region, respectively, and the gradient starting point and the gradient end point correspond to the gradient region of the effective rod length. The ends of the first sub-region and the tail terminal region that are separated are respectively the first inflection point and the second inflection point. The total rod length of the preform rod body (mother rod) corresponds to the distance between the first inflection point and the second inflection point.
[0068] Among them, each of the reaction gases includes at least one of SiCl4, O2, GeCl4, POCl3, C2F6 and BCl3. Among the above gases, some gases are main deposition gases, such as SiCl4 and O2; some gases can improve the profile parameters and mechanical properties of the preform rod (mother rod), such as GeCl4, POCl3, C2F6 and BCl3, etc., and can be appropriately adjusted during the actual production process.
[0069] The geometric dimensions of the areas (first sub-area and the tail terminal area) near the two ends of the preform rod body (mother rod) are generally small, and the closer to the edge, the smaller. The flow rate of Si and O precursors (such as SiCl4 and O2) is controlled by the air intake control structure 3 to increase. Specifically, the flow rate of the reaction gas is controlled by the air intake control structure 3 as the position of the excitation source 4 changes. In the first sub-area, the reaction gas gradually increases from the gradual starting point to the first inflection point. In the tail terminal area, the reaction gas gradually decreases from the second inflection point to the gradual end point, and the concentration of the reaction gas in the first sub-area and the tail terminal area is increased to increase the deposition rate of the reaction gas, ensuring that the geometric dimensions of the two ends are equivalent to the area of the effective rod length in the middle. In this process, the power of the matching excitation source 4 can also be increased slightly to speed up the reaction efficiency of the reaction gas. It should be noted that the ratio of O2 to SiCl4 needs to be greater than 2, preferably greater than 2.5, needs to be less than 6, and more preferably needs to be less than 5. If the power of the excitation source 4 is changed, the power increment of the excitation source 4 is equivalent to the increase in the amount of the reaction gas. If the increase in the flow rate of the reaction gas is less than 5%, the power of the excitation source 4 may not be changed. Alternatively, only the flow rate of SiCl4 may be increased, but the ratio of O2 to SiCl4 cannot be lower than 2.5. For the effective rod length region in the middle, the core diameter distribution is not completely straight. The core diameter can be compensated by controlling the flow rate of the reaction gas through the intake control structure 3, so as to achieve a longer effective rod length, such as Figure 5 As shown, in the first sub-zone and the tail terminal zone, the flow rate of the reaction gas increases continuously and gradually during the process of the reaction gas corresponding to the excitation source 4 moving to the first inflection point and the second inflection point, and the core diameter deviation of the embodiment is obviously better than that of the comparison example, so it is beneficial to improve the consistency of the radial parameters of the entire preform rod body (mother rod).
[0070] Wherein, when the reaction gas includes SiCl4 and O2, the increase of the reaction gas is 1% to 20%.
[0071] During the deposition process, the incomplete reaction of the first sub-region and the tail terminal region at both ends will form a dust ring on the inner wall of the quartz tube 2, which is prone to breakage during the deposition and melting process. The breakage of the dust ring is due to the difference in expansion coefficient between the doped silica and the pure silica liner. The positive dopant has a greater impact on the expansion coefficient. By reducing the positive dopant Ge or P precursor (such as GeCl4 or POCl3), the overall strength of the first sub-region and the tail terminal region can be improved. Specifically, the flow rate of the reaction gas is controlled by the intake control structure 3 as the position of the excitation source 4 changes. In the first sub-region, the reaction gas gradually decreases from the gradual starting point to the first inflection point. In the tail terminal region, the reaction gas gradually increases when moving from the second inflection point to the gradual end point. In this process, the reduction of the reaction gas is 30% to 100%.
[0072] The distance from the starting point of the gradual change to the first inflection point is 20 mm to 200 mm, and the distance from the second inflection point to the end point of the gradual change is 20 mm to 190 mm. Considering that the gas moves from the feed end to the discharge end of the quartz tube 2, the positions of the starting point of the gradual change and the end point of the gradual change do not overlap when necessary. The distance from the starting point of the gradual change to the first inflection point is greater than the distance from the end point of the gradual change to the second inflection point, because the gas flows toward the discharge end of the quartz tube 2 and needs to reach a stable state in advance.
[0073] The reaction efficiency of the part near the feed end of the quartz tube 2 is not as good as that of the area near the discharge end of the quartz tube 2 because the reaction gas is still in the process of being heated and excited. Its cross-sectional refractive index is not high, and generally shows a trend of gradually increasing from the feed end to the discharge end and then remaining stable. At this time, the axial compensation of the refractive index can be achieved by increasing the flow rate of the Ge and P precursors near the feed end.
[0074] Due to the incomplete reaction in the first sub-region and the tail terminal region, the doping efficiency is low, especially the negative dopant used to react to form the sunken cladding, which may lead to large additional loss in macrobending. In order to solve this problem, the concentration of negative dopants, such as C2F6 or BCl3, can be appropriately increased in the above-mentioned area, and gradually increased in the first sub-region and the tail terminal region. Specifically, the flow rate of the reaction gas is controlled by the intake control structure 3 as the position of the excitation source 4 changes. In the first sub-region, the reaction gas gradually increases from the gradual starting point to the first inflection point. In the tail terminal region, the reaction gas gradually increases from the gradual end point to the second inflection point, and the increase is 2% to 50%, so as to achieve compensation for negative doping and ensure that the anti-bending at both ends can meet the requirements.
[0075] The total length of the preform (mother rod) is L total , the Ltotal ≥500mm, the length of the first sub-area and the tail terminal area are both L, 0.03L total ≤L≤0.05L total ; Among the plurality of sub-areas, at least one sub-area in which the reaction gas flow rate remains constant, and the length of the sub-area is set to L m , L m ≥ 0.2 L total .
[0076] The continuous change control of a certain reaction gas component in the multiple sub-areas can be controlled by a single flow meter, changing from the starting flow to the target flow along the position. In addition, for the reaction gas with reduced flow, the continuous change control in the corresponding sub-area can be controlled by two flow meters in series, one of which changes normally and the other is feedback controlled based on the axial position of the excitation source 4. In addition, for the reaction gas with increased flow, the continuous change control in the corresponding sub-area uses two flow meters in parallel, one of which changes normally and the other is feedback controlled based on the axial position of the excitation source 4. The relevant flow meter uses a high-precision mass flow controller 33, whose response time is less than 200ms, which can achieve more precise control.
[0077] Generally speaking, the parameters of the first sub-area and the tail terminal area fluctuate greatly due to the movement return of the excitation source 4 or the feeding and discharging of the quartz tube 2. The parameter change trends of the intermediate area are different due to the actual equipment and process parameters. Therefore, the preform body (mother rod) can be axially divided into three areas for doping compensation. In the case of significant axial fluctuations of some intermediate parameters, they can be further subdivided.
[0078] like Figure 2 As shown in the figure, the entire preparation process of this scheme includes, according to the mother rod test, the zoning judgment is made according to the profile parameters, according to the axial change of the profile parameters in the sub-area, the axial change of the feed flow rate is calculated, and the core rod is prepared according to the above control parameters. The prepared core rod is tested again as a mother rod, and the drawing can be carried out if the parameters and the effective rod length are qualified; if it is unqualified, the axial change trend of the feed flow rate at the feed end is adjusted again based on the new mother rod test results. After drawing, the axial change trend of the feed flow rate can also be further adjusted according to the output ratio of qualified optical fiber, the optical fiber test results and its location. In general, the core rod test results are used as the mother rod adjustment control parameters, and the optical fiber drawing results are used as auxiliary judgments. In the daily production process, each reel of optical fiber will be tested, so the axial change trend of the feed flow rate can be adjusted according to the optical fiber test results. When the output ratio of qualified optical fiber meets the production requirements, continuous and stable production can be carried out according to the optimal parameters.
[0079] It should be noted that the determination of the optimal parameters may require iterative production optimization of multiple mother rods. During this process, multiple mother rods need to be tested to gradually optimize the production parameters and obtain the final mapping relationship between the position of the excitation source 4 and the intake control structure 3, that is, the optimal production parameters. In the subsequent production process, production can be directly carried out with the current optimal production parameters.
[0080] like Figures 3 to 5 As shown, the comparative example adopts a constant feed flow rate of the reaction gas, while the embodiment adjusts the flow rate of the reaction gas at the feed end of the quartz tube 2 through the intake control structure 3 according to the axial position of the excitation source 4, as shown in FIG. Figure 3 As shown, the first sub-area and the tail terminal area are used to reduce the doping of germanium at both ends to avoid breakage. The middle sub-area two and sub-area four are used to increase the Δ of the core rod and increase the proportion of qualified optical fibers, and the sub-area three remains unchanged.
[0081] like Figure 4 As shown, for F doping, especially the sunken cladding, in order to ensure the bending strength of the optical fiber, it can be deeper, so the F doping is appropriately increased at both ends of the first sub-area and the tail terminal area, which is beneficial to improve the bending strength of the first sub-area and the tail terminal area, and increase the proportion of qualified optical fibers. The deeper part on the left side of the middle sub-area 2 can be ignored and divided into one sub-area.
[0082] Through the above method, when the excitation source 4 is located at different positions on the axis of the quartz tube 2, the corresponding reaction gas flow rate is controlled by the air intake control structure 3, so as to realize the compensation regulation of the refractive index deviation of the mother rod, significantly reduce the deviation of the profile parameters at both ends, and prepare a core rod with a profile close to the ideal profile in a longer axial area, especially the change slope of the left and right ends is significantly reduced, thereby increasing the effective rod length and the output ratio of qualified optical fiber, which has excellent application value.
[0083] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing an optical fiber preform rod by an in-tube method, comprising a preparation device, wherein the preparation device comprises a rotating mounting structure, a quartz tube, an excitation source and an air intake control structure, wherein the rotating mounting structure is used to fix the quartz tube and drive the quartz tube to rotate around its axis, the air intake control structure is arranged at the air intake end of the quartz tube and is used to control the flow rate of the reaction gas at the air intake end of the quartz tube, the excitation source has a movement stroke along the axis direction of the quartz tube and is used to promote the reaction gas to produce chemical deposition in the quartz tube, and the method for preparing an optical fiber preform rod by an in-tube method comprises the following preparation processes: Under preset deposition conditions, the quartz tube is mounted on the rotating mounting structure, the excitation source is controlled to reciprocate along the axis direction of the quartz tube, each of the reaction gases is introduced into the quartz tube through the gas inlet control structure, and the reaction gas is chemically deposited in the quartz tube by the excitation source to form a preformed rod body; It is characterized in that There are m sub-regions with m+1 axial points divided along the axial direction of the preform rod, and the flow opening of the air intake control structure is calibrated according to the cross-sectional parameters and bending strength parameters at each axial point to adjust the continuous change of the flow of each reaction gas in each sub-region.
2. The method for preparing an optical fiber preform rod by the in-tube method according to claim 1, It is characterized in that The plurality of sub-regions are divided according to the cross-sectional parameters and the bending strength of the preform body, and the cross-sectional parameters in each sub-region gradually increase or decrease or remain substantially unchanged.
3. The method for preparing an optical fiber preform by the in-tube method according to claim 2, It is characterized in that The plurality of sub-areas include a first sub-area at the feed end of the quartz tube and a tail terminal area at the discharge end of the quartz tube, the first sub-area and the end corresponding to the tail terminal area are the gradient starting point and the gradient end point, respectively, and the first sub-area and the end separated from the tail terminal area are the first inflection point and the second inflection point, respectively; The excitation source moves between the first inflection point and the second inflection point, and the total length of the preformed rod is L total , the L total is the distance between the first inflection point and the second inflection point; and / or, The spacing between the multiple axial points is L b , the L b ≤20mm.
4. The method for preparing an optical fiber preform by the in-tube method according to claim 3, It is characterized in that The reaction gas includes SiCl 4 and O 2 ; In the first sub-zone, the reaction gas gradually increases from the gradual change starting point to the first inflection point; and\or, In the tail terminal region, the reaction gas gradually decreases from the second inflection point to the gradual end point.
5. The method for preparing an optical fiber preform rod by the in-tube method according to claim 4, It is characterized in that In the first sub-area, the reaction gas gradually increases from the gradual starting point to the first inflection point, and the increase rate of the reaction gas is 1% to 20%; and\or, Each of the reaction gases includes SiCl 4 , O 2 、GeCl 4 POCl 3 , C 2 F 6 and BCl 3 At least one of .
6. The method for preparing an optical fiber preform by the in-tube method according to claim 3, It is characterized in that The reaction gas includes GeCl 4 or POCl 3 ; In the first sub-zone, the reaction gas gradually decreases from the gradual change starting point to the first inflection point; and\or, In the tail terminal region, the reaction gas gradually increases when moving from the second inflection point to the gradual end point.
7. The method for preparing an optical fiber preform by the in-tube method according to claim 6, It is characterized in that In the first sub-area, the reaction gas gradually decreases from the gradual change starting point to the first inflection point, and the reduction range of the reaction gas is 10% to 100%; and / or, The distance from the gradual change starting point to the first inflection point is 20 mm to 200 mm, and the distance from the second inflection point to the gradual change end point is 20 mm to 190 mm.
8. The method for preparing an optical fiber preform rod by the in-tube method according to claim 3, It is characterized in that The reaction gas includes C 2 F 6 or BCl 3 ; In the first sub-zone, the reaction gas gradually increases from the gradual change starting point to the first inflection point; and\or, In the tail terminal region, the reaction gas gradually increases from the gradual end point to the second inflection point.
9. The method for preparing an optical fiber preform rod by the in-tube method according to claim 3, It is characterized in that In the first sub-area, the reaction gas gradually increases from the gradual change starting point to the first inflection point, and the increase rate of the reaction gas is 2% to 50%; and / or, In the tail terminal region, the reaction gas gradually increases from the gradual end point to the second inflection point, and the increase rate of the reaction gas is 2% to 50%.
10. The method for preparing an optical fiber preform rod by the in-tube method according to claim 1, It is characterized in that The L total ≥500mm, the length of the first sub-area and the tail terminal area are both L, 0.03L total ≤L≤0.05L total ; and\or, Among the plurality of sub-areas, at least one sub-area in which the reaction gas flow rate remains constant, and the length of the sub-area is set to L m , L m ≥ 0.2 L total .
Citation Information
Cited By
Method for preparing optical fiber preform through in-tube method
CN118908558A