Purple pigment for glass printing ink and preparation method thereof

By mixing cobalt-magnesium precursors with boric acid and controlling calcination conditions, a purple pigment matching glass powder was prepared, solving the problem of purple pigment decomposition or turning blue in glass inks, achieving a bright purple color effect, and suitable for industrial production.

CN118908562APending Publication Date: 2024-11-08FULLN GLAZE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410972324.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The purple pigment in existing glass inks decomposes or turns blue during high-temperature sintering, and cannot produce a bright purple hue.

Method used

A purple pigment with high chemical homogeneity, fine particles, and compatibility with glass powder was prepared by mixing cobalt-magnesium precursors with boric acid and controlling the molar ratio and calcination temperature. Sodium hydroxide was used as a precipitant and the mixture was pulverized by air jet milling to control particle size and dispersibility.

Benefits of technology

The prepared purple pigment exhibits pure color and a distinct purple hue in glass inks, and is suitable for large-scale mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908562A_ABST
    Figure CN118908562A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: preparing a mixed supersaturated solution from cobalt nitrate and magnesium nitrate in proportion, adding a precipitant solution to prepare a precursor precipitate containing cobalt and magnesium, carrying out suction filtration, washing and drying treatment to obtain a cobalt and magnesium precursor, mixing the cobalt and magnesium precursor with boric acid in proportion, putting the mixture into a kiln, and calcining at 800-950 DEG C to obtain the purple pigment for glass printing ink. The purple pigment prepared by crushing, powdering, washing and drying is pure in color in the glass ink, has more obvious purple hue and brighter color, and the preparation method is simple, easy to operate and suitable for large-scale batch production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pigments, and in particular to a purple pigment for glass ink and a preparation method thereof. Background Art

[0002] Glass ink is a special ink that is screen-printed on the glass surface. It is composed of glass powder, colorant and solvent. After high-temperature firing, it is firmly bonded to the glass. The type of colorant determines the coloring type of the glass ink.

[0003] Since the sintering temperature of glass ink is around 550-720°C, the glass powder of glass ink contains a large amount of low-melting-point flux substances, such as bismuth-boron-silicon low-melting-point glass, high-lead boron glass, etc. These low-melting-point flux components will cause most of the purple pigment components to decompose or fail to present a bright purple hue.

[0004] Common types of purple inorganic pigments include cobalt phosphate, lithium cobalt phosphate, neodymium aluminum violet, cobalt silicon violet, chrome tin violet, etc. These pigments do not show color in glass inks or show a blue hue and lose the purple hue of the pigment itself. Summary of the invention

[0005] In view of the defects of the above-mentioned prior art, one of the objects of the present invention is to provide a method for preparing a purple pigment for glass ink, which is simple and easy to operate. The second object of the present invention is to provide a purple pigment for glass ink, which can present bright colors and pure tones in glass ink and meet the printing requirements of glass ink.

[0006] One of the purposes of the present invention is achieved by the following technical solution:

[0007] A method for preparing a purple pigment for glass ink comprises the following steps:

[0008] 1) weighing cobalt nitrate and magnesium nitrate according to a molar ratio of n(Co):n(Mg)=(0.4-0.65):(0.35-0.6), mixing and dissolving the cobalt nitrate and magnesium nitrate in water to prepare a mixed supersaturated solution;

[0009] 2) Add 2-4 mol / L sodium hydroxide aqueous solution dropwise into the above mixed supersaturated solution using a dropping funnel, and continue stirring until no more precipitation occurs in the reaction solution;

[0010] 3) taking the above precipitate, filtering, washing and drying it to obtain a cobalt-magnesium precursor mixture;

[0011] 4) uniformly mixing the cobalt-magnesium precursor mixture and boric acid according to mass percentage to obtain a mixed raw material, wherein the ratio of the cobalt-magnesium precursor mixture is 45-55%, and the ratio of the boric acid is 45-55%;

[0012] 5) The mixed raw material is calcined at 800-950° C. for 3-4 hours, and then crushed, pulverized, washed and dried to finally obtain a purple pigment for glass ink.

[0013] In the above preparation process, the content of each component can be accurately controlled, the components can be fully mixed, and the introduction of harmful substances that are detrimental to the material properties can be avoided. The produced pigment powder has high chemical uniformity, fine particle size, and narrow particle size distribution. At the same time, the equipment and process required for preparation are relatively simple, which is convenient for industrial production.

[0014] Preferably, the sum of the molar ratios of n(Co) and n(Mg) is one molar unit.

[0015] Preferably, in step 3), the drying temperature is 75-85°C.

[0016] Preferably, in step 4), the mass percentage of the cobalt-magnesium precursor mixture is 55%, and the mass percentage of boric acid is 45%.

[0017] Preferably, in step 5), the calcination heating time is 8 to 9 hours.

[0018] Using sodium hydroxide as a precipitant, the obtained cobalt-magnesium precursor mixture has high chemical activity, low sample sintering temperature, stable performance and good reproducibility. By strictly controlling the dripping conditions of the precipitant and the heating time and insulation time of the calcination, the purity, particle size, grain size and dispersibility of the obtained pigment powder can be controlled.

[0019] Preferably, in step 5), the pulverization treatment is carried out by air jet milling, and the fineness of the purple pigment for glass ink is controlled to be less than 0.05% under a 400-mesh sieve.

[0020] Preferably, in step 5), the drying temperature is 120-150°C.

[0021] Preferably, in step 5), after drying, the water content of the purple pigment for glass ink is less than 0.1%.

[0022] The second object of the present invention is achieved by adopting the following technical solution:

[0023] A purple pigment for glass ink is prepared by the preparation method of the purple pigment for glass ink.

[0024] The beneficial effects of the present invention are as follows: compared with common inorganic purple pigments, the purple pigment prepared by the present invention is pure in color in glass ink, has a more obvious purple hue, and is more vivid in color; the preparation method is simple, easy to operate, and suitable for large-scale batch production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a comparison chart of the coloring effects of comparative example 1 and example 1 in glass ink;

[0026] Figure 2 This is a comparison chart of the coloring effects of comparative example 2 and example 1 in glass ink;

[0027] Figure 3 is the XRD pattern of Example 1;

[0028] Figure 4 is the XRD pattern of Comparative Example 1;

[0029] Figure 5 This is the XRD pattern of Comparative Example 2. DETAILED DESCRIPTION

[0030] The following are specific embodiments of the present invention. Unless otherwise specified, the raw materials, equipment, etc. used in the following embodiments can be obtained by purchase.

[0031] The raw materials were weighed according to the ratio in Table 1, and purple pigments for glass inks of different embodiments were obtained according to the preparation method in Table 1. The details are shown in Table 1:

[0032] Table 1 Experimental parameters used in Examples 1 to 4

[0033]

[0034] In Table 1, the preparation method of purple pigment for glass ink comprises the following steps:

[0035] 1) cobalt nitrate and magnesium nitrate were weighed according to the molar ratio, directly mixed and dissolved in deionized water, and rapidly stirred at room temperature at a stirring speed of 2000-2500 r / min to obtain a mixed supersaturated solution;

[0036] 2) preparing sodium hydroxide into a 2 mol / L sodium hydroxide aqueous solution, adding the sodium hydroxide aqueous solution dropwise into the above mixed supersaturated solution using a dropping funnel, and continuously stirring the reaction solution until no more precipitation continues to precipitate in the reaction solution;

[0037] 3) taking the above precipitate, filtering it twice, washing it twice and drying it, to obtain a cobalt-magnesium precursor mixture, the drying temperature being 80° C.;

[0038] 4) mixing the cobalt-magnesium precursor mixture and boric acid in a mass percentage of 55% and 45% to obtain a mixed raw material;

[0039] 5) The mixed raw material is sintered at 900°C for 3h, wherein the calcination heating time is 8h, and then pulverized by air jet mill, and the fineness is controlled to be less than 0.05% under a 400-mesh sieve; and then washed twice with water to remove unreacted soluble salts, and then dried at 130°C to finally obtain a purple pigment for glass ink, wherein the water content of the purple pigment for glass ink is less than 0.1%.

[0040] Comparative Example 1

[0041] Comparative Example 1 provides a chrome tin violet pigment, and its preparation method comprises the following steps: according to weight parts, 50 parts of tin oxide, 25 parts of calcium carbonate, 18 parts of quartz, 3 parts of chrome green, and 4 parts of borax are evenly mixed in a mixer, and after powdering to make the raw materials fully contact with each other, calcining is carried out at a calcination temperature of 1260-1280°C and a heat preservation time of 3h, and then crushing and air flow pulverizing are carried out, and after passing through a 400-mesh sieve, the chrome tin violet pigment is obtained.

[0042] Comparative Example 2

[0043] Comparative Example 2 provides a silicon cobalt violet pigment, and its preparation method includes the following steps: 55 parts of cobalt oxide and 45 parts of quartz are evenly mixed in a mixer according to weight parts, and after powdering to make the raw materials fully contact with each other, calcining is carried out at a calcination temperature of 1280-1300°C and a holding time of 3 hours, and then crushing and air flow pulverizing are carried out, and after passing through a 400-mesh sieve, the silicon cobalt violet pigment is obtained.

[0044] The pigments prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were dry-pressed into round cake-shaped samples, and chromaticity tests were performed using a Japanese Konica Minolta CM-3700D. The measured chromaticity data values ​​are shown in Table 2, wherein the chromaticity data are characterized by Lab values, with L values ​​ranging from 0 to 100, indicating lightness values; a values ​​ranging from -128 to +127, indicating a range from green to red; and b values ​​ranging from -128 to +127, indicating a range from blue to yellow.

[0045] Table 2 Chroma test results of the pigments obtained in Examples 1 to 4 and Comparative Examples 1 to 2

[0046]

[0047]

[0048] As can be seen from Table 1, compared with the chrome tin violet pigment of Comparative Example 1 and the silicon cobalt violet pigment of Comparative Example 2, the purple pigments prepared in Examples 1 to 4 are brighter in color, have a more obvious purple hue, and are more vivid in color.

[0049] The pigments obtained in Example 1, Comparative Example 1 and Comparative Example 2 are colored in silicon-boron system glass ink. In terms of mass ratio, the silicon-boron system glass ink includes 60% silicon-boron system glass powder, 15% varnish and 25% pigment. The coloring effects of Comparative Example 1 and Example 1 are shown in FIG. Figure 1 The coloring effect of comparative example 2 and example 1 is shown in Figure 2 .

[0050] from Figure 1 and Figure 2 It can be seen that, compared with Comparative Examples 1 and 2, Example 1 can present a more obvious purple tone in the silicon-boron system glass ink, and the color is also brighter.

[0051] Figure 3 is the XRD pattern of Example 1, Figure 4 is the XRD diagram of Comparative Example 1, Figure 5 This is the XRD pattern of Comparative Example 2. Figure 3 No cobalt phase was detected in Example 1. This may be because during the sintering process, cobalt replaced the position of magnesium in magnesium borate in the form of doping. Figure 1 and Figure 2 From the color of Example 1, it can be seen that Example 1 is a cobalt magnesium borate purple pigment containing a cobalt, magnesium, and boric acid system. Example 1 matches the glass powder component in the glass ink and can be perfectly integrated with the low melting point flux in the glass powder during sintering. The low melting point flux will not affect the purple pigment component of Example 1 during sintering, and therefore will not affect the color of Example 1. Figure 4 and Figure 5 It can be seen that Comparative Example 1 is a chrome tin violet pigment, and Comparative Example 2 is a silicon cobalt violet pigment.

[0052] Based on the property that glass powder in glass ink contains a large amount of low melting point substances, the invention selects components matching the glass powder in glass ink. Compared with common inorganic purple pigments, the purple color of the invention is purer and can present a brighter purple tone in glass ink.

[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should fall within the protection scope of the present invention.

Claims

1. A method for preparing a purple pigment for glass ink, characterized in that: The following steps are involved: 1) Weigh cobalt nitrate and magnesium nitrate according to a molar ratio of n(Co):n(Mg)=(0.4-0.65):(0.35-0.6), mix and dissolve the cobalt nitrate and magnesium nitrate in water to prepare a mixed supersaturated solution; 2) Add 2-4 mol / L sodium hydroxide aqueous solution dropwise into the above mixed supersaturated solution using a dropping funnel, and continue stirring until no more precipitation occurs in the reaction solution; 3) taking the above precipitate, filtering, washing and drying it to obtain a cobalt-magnesium precursor mixture; 4) The cobalt-magnesium precursor mixture and boric acid are uniformly mixed according to mass percentage to obtain a mixed raw material, wherein the ratio of the cobalt-magnesium precursor mixture is 45-55%, and the ratio of the boric acid is 45-55%; 5) The mixed raw material is calcined at 800-950° C. for 3-4 hours, and then crushed, pulverized, washed and dried to finally obtain a purple pigment for glass ink.

2. The method for preparing a purple pigment for glass ink according to claim 1, characterized in that: In step 3), the drying temperature is 75-85°C.

3. The method for preparing a purple pigment for glass ink according to claim 1, characterized in that: In step 4), the mass percentage of the cobalt-magnesium precursor mixture is 55%, and the mass percentage of boric acid is 45%.

4. The method for preparing a purple pigment for glass ink according to claim 1, characterized in that: In step 5), the calcination heating time is 8 to 9 hours.

5. The method for preparing a purple pigment for glass ink according to claim 1, characterized in that: In step 5), the powdering treatment is carried out by air jet milling, and the fineness of the purple pigment for glass ink is controlled to be less than 0.05% under a 400-mesh sieve.

6. The method for preparing a purple pigment for glass ink according to claim 1, characterized in that: In step 5), the drying temperature is 120-150°C.

7. The method for preparing a purple pigment for glass ink according to claim 6, characterized in that: In step 5), after drying, the water content of the purple pigment for glass ink is less than 0.1%.

8. A purple pigment for glass ink, characterized in that: The invention is prepared by the method for preparing the purple pigment for glass ink according to any one of claims 1 to 7.