Glass powder for fine grid silver paste of high-sheet-resistance TOPCon battery as well as preparation method and application of glass powder

By optimizing the glass powder composition and preparation process, the problems of low contact resistance and high open-circuit voltage of high sheet resistance N-type TOPCon cells under LECO sintering technology were solved, achieving high photoelectric conversion efficiency and stability, and making it suitable for the preparation of fine grid silver paste for high sheet resistance TOPCon cells.

CN118908579APending Publication Date: 2024-11-08FOSHAN HAOYU XINNENG TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410973693.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing glass powders cannot meet the application requirements of high sheet resistance N-type TOPCon cells under LECO sintering technology, and cannot simultaneously achieve low contact resistance and high open circuit voltage. Furthermore, traditional silver-aluminum pastes may lead to metal composites and reduced cell efficiency.

Method used

A glass powder for fine grid silver paste in high sheet resistance TOPCon batteries is provided. By optimizing the addition amounts of sodium oxide, aluminum oxide, silicon oxide, zinc oxide, lead oxide, boron oxide, and lithium oxide, and adding tellurium oxide, selenium oxide, and tungsten oxide as regulators, combined with LECO sintering technology, good ohmic contact and high open circuit voltage are ensured at low sintering temperature. The glass powder with a D50 particle size of 1.8 to 2 μm is obtained by high-temperature melting in a platinum crucible, grinding in a planetary ball mill, and secondary grinding in an air jet mill.

Benefits of technology

LECO sintering technology achieves good ohmic contact between the silver electrode and the high sheet resistance silicon substrate of the battery, reducing contact resistance, improving photoelectric conversion efficiency, reducing metal recombination, and enhancing battery efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of H01B1 / 16, in particular to glass powder for high-sheet-resistance TOPCon battery fine grid silver paste and a preparation method and application thereof.The glass powder is at least prepared from, by weight, 1-10 parts of sodium oxide, 2-15 parts of aluminum oxide, 3-25 parts of silicon oxide, 5-15 parts of zinc oxide, 65-85 parts of lead oxide, 5-20 parts of boron oxide, 1-5 parts of lithium oxide and 1-10 parts of oxide modifier; the preparation method is better matched with the technological characteristics of an LECO sintering technology and a high-sheet-resistance TOPCon battery, and has extremely important research value and practical application value for further improving the efficiency of the N-type TOPCon battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of H01B1 / 16, and in particular to a glass powder for high-square-resistance TOPCon battery fine grid silver paste, and a preparation method and application thereof. Background Art

[0002] With the increasing severity of energy shortages and environmental pollution, sustainable new energy projects have received the attention of countries around the world. The photovoltaic energy storage industry has become an indispensable part of my country's energy structure. With the advancement of related technologies, the mainstream PERC (passivated emitter and rear cell technology) monocrystalline cells on the market have gradually been replaced by high-efficiency N-type TOPCon solar cells (tunneling oxide passivated contact cells). TOPCon solar cells have further improved the open circuit voltage, short circuit current and fill factor of the cell through the improvement of related technologies, achieving a significant increase in cell efficiency. With the iteration of technology, the industry has begun to promote the use of the new LECO (laser enhanced contact optimization) sintering technology to replace the traditional high-temperature sintering technology. This move will truly realize the aluminum-free conductive silver paste on the front of the TOPCon cell. Traditional high-temperature sintering not only damages the cell but also easily causes more serious metal-induced recombination, which will greatly reduce the efficiency of the cell. In order to obtain good ohmic contact between the front silver electrode and the silicon substrate, the original TOPCon cell usually uses aluminum-containing silver paste for printing and sintering. The introduction of aluminum can easily lead to the generation of "aluminum thorns" and thus destroy the PN junction, and also bring about many adverse effects such as the aggravation of metal recombination. However, with the help of LECO sintering technology, the use of aluminum-free silver paste on the front of the TOPCon battery can be achieved, which can balance the open circuit voltage and fill factor, and thus obtain a higher open circuit voltage and fill factor. The LECO process is to irradiate the battery cell with high-intensity laser and apply a bias voltage of 10V or more at the same time. The resulting local current of several amperes will significantly reduce the contact resistance between the metal and the semiconductor. The essence of the LECO process is actually to enhance the contact ability of the silver paste with the battery or circuit, reduce the contact resistance, and minimize the damage to the passivation layer of the battery cell. These factors can greatly improve the photoelectric conversion efficiency of crystalline silicon cells, and can achieve a conversion efficiency increase of about 0.2 to 0.6%. N-type TOPCon cells are also developing towards higher battery square resistance. High square resistance batteries can reduce the recombination of photogenerated carriers and reduce the defect density of the battery, which is conducive to increasing the open circuit voltage of the battery and further improving the battery efficiency. However, the current glass powder cannot meet the above application requirements. For example, a Chinese patent (publication number CN114213026A) discloses a composite system glass powder for silver paste of the secondary grid electrode of a crystalline silicon solar cell. Although the contact resistance is reduced and the open circuit voltage of the battery is increased by optimizing the glass powder system, further improvement is still needed to meet the application requirements of high square resistance batteries under the LECO process. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a glass powder for fine grid silver paste of high square resistance TOPCon battery, which better matches LECO sintering technology and the process characteristics of high square resistance TOPCon battery, and has extremely important research value and practical application value for further improving the efficiency of N-type TOPCon battery.

[0004] On the one hand, the present invention provides a glass powder for high square resistance TOPCon battery fine grid silver paste. The raw materials for preparing the glass powder include at least, by weight: 1-10 parts of sodium oxide, 2-15 parts of aluminum oxide, 3-25 parts of silicon oxide, 5-15 parts of zinc oxide, 65-85 parts of lead oxide, 5-20 parts of boron oxide, 1-5 parts of lithium oxide, and 1-10 parts of an oxide regulator.

[0005] As a preferred technical solution, the oxide regulator is selected from at least one of tellurium oxide, selenium oxide, barium oxide, tungsten oxide, and calcium oxide. Preferably, the oxide regulator is selected from any one of tellurium oxide, selenium oxide, and tungsten oxide.

[0006] As a preferred technical solution, based on the total weight of the glass powder, the added amount of the sodium oxide is 1.00% to 3.00%, preferably 1.00% to 1.50%.

[0007] As a preferred technical solution, based on the total weight of the glass powder, the added amount of the aluminum oxide is 3.00% to 5.00%, preferably 3.50% to 4.20%.

[0008] As a preferred technical solution, based on the total weight of the glass powder, the added amount of silicon oxide is 5.00% to 10.00%, preferably 5.56% to 6.88%.

[0009] As a preferred technical solution, based on the total weight of the glass powder, the added amount of zinc oxide is 5.00% to 8.00%, preferably 6.00% to 6.32%.

[0010] As a preferred technical solution, based on the total weight of the glass powder, the added amount of lead oxide is 65.00% to 75.00%, preferably 65.00% to 71.50%.

[0011] As a preferred technical solution, based on the total weight of the glass powder, the added amount of the boron oxide is 8.00% to 15.00%, preferably 8.50% to 10.50%.

[0012] As a preferred technical solution, based on the total weight of the glass powder, the added amount of the lithium oxide is 1.00% to 2.00%, preferably 1.00% to 1.50%.

[0013] As a preferred technical solution, based on the total weight of the glass powder, the added amount of the lithium oxide is 2.00% to 8.00%, preferably 2.00% to 6.00%.

[0014] The glass powder provided by the present invention is optimized based on the LECO sintering technology. By optimizing the addition amounts of sodium oxide, aluminum oxide, silicon oxide, zinc oxide, lead oxide, boron oxide and lithium oxide in the glass powder system, under the cooperation of oxide regulators such as tellurium oxide, selenium oxide and tungsten oxide, the provided glass powder has appropriate etching ability and high-temperature melting characteristics, and has moderate etching ability for the passivation layer of the battery cell, reducing the recombination caused by the sintering of silver paste on the battery surface, ensuring that under the condition of the lower sintering temperature (690-730°C) of the LECO sintering technology, the silver electrode can still form a good ohmic contact with the high-square-resistance battery silicon substrate while maintaining a higher open circuit voltage, thereby effectively improving the photoelectric conversion efficiency of the TOPCon battery.

[0015] On the other hand, the present invention provides a method for preparing glass powder for high square resistance TOPCon battery fine grid silver paste, which comprises at least the following steps: placing sodium oxide, aluminum oxide, silicon oxide, zinc oxide, lead oxide, boron oxide, lithium oxide, and an oxide regulator in a mixer, transferring them to a platinum crucible after mixing, placing the crucible in a sintering furnace at 1000-1100°C, and smelting at high temperature for 20-40 minutes, then taking the crucible out of the sintering furnace and placing the melt in the crucible on a cooling roller for cold rolling treatment, placing the product after cold rolling treatment in a ball mill for ball milling treatment, screening the ball milled product, and then performing secondary grinding treatment to obtain glass powder.

[0016] As a preferred technical solution, the ball mill is a planetary ball mill.

[0017] As a preferred technical solution, the D50 particle size of the glass powder is 1.8-2 μm.

[0018] As a preferred technical solution, the mass ratio of the grinding balls in the ball milling process to the product after the cold rolling process is (3-6): 1, preferably 5: 1. The grinding balls do not need to be particularly limited, and any grinding balls in the art can be used.

[0019] As a preferred technical solution, the ball milling speed of the ball milling treatment is 150-300 rpm, and the ball milling time is 90-180 min.

[0020] As a preferred technical solution, the screening is performed using a 200-250 mesh sieve.

[0021] As a preferred technical solution, the secondary grinding treatment is carried out by using a jet mill, the pressure of the jet mill is 0.8-1.2 MPa, and the secondary grinding treatment time is 10-30 min.

[0022] Furthermore, the present invention adopts a platinum crucible for high-temperature smelting to effectively avoid the adverse effects of impurities in the crucible on the glass during the smelting process, further optimizes the screening after grinding with a planetary ball mill, and after screening, uses a jet mill for secondary grinding to obtain glass powder with a D50 particle size of 1.8 to 2 μm, so that the powder maintains a good glassy structure, thereby ensuring the stability of subsequent applications.

[0023] A third aspect of the present invention provides an application of glass powder for high-square-resistance TOPCon battery fine grid silver paste, which is applied to the preparation of high-square-resistance TOPCon battery fine grid silver paste.

[0024] As a preferred technical solution, the amount of glass powder added to the high square resistance TOPCon battery fine grid silver paste is 1.5-3.0wt%.

[0025] As a preferred technical solution, the raw materials for preparing the high square resistance TOPCon battery fine grid silver paste at least include glass powder, silver powder, organic carrier and organic solvent.

[0026] Preferably, the organic carrier is selected from at least one of epoxy resin, acrylic resin and ethyl cellulose.

[0027] Preferably, the solvent is selected from at least one of hexadecene alcohol, terpineol, silicone oil and diethylene glycol dibutyl ether.

[0028] Preferably, the mass ratio of the silver powder, glass powder, organic carrier and solvent is (88-90):(1.5-3.0):(6-10):(2-5).

[0029] In addition, compared with the traditional N-type TOPCon front silver-aluminum paste glass powder, the glass powder provided by the present invention has a lower addition amount in the conductive silver paste and can meet the requirements of low contact resistance, high open circuit voltage and high photoelectric conversion efficiency on high square resistance TOPCon batteries, which greatly reduces the amount of glass powder used and truly removes metal aluminum, reduces unnecessary metal composites, and promotes the improvement of battery efficiency.

[0030] Beneficial Effects

[0031] 1. The present invention provides a glass powder for fine grid silver paste of high square resistance TOPCon battery, which better matches the LECO sintering technology and the process characteristics of high square resistance TOPCon battery, and has extremely important research value and practical application value for further improving the efficiency of N-type TOPCon battery.

[0032] 2. The glass powder provided by the present invention is optimized based on the LECO sintering technology. By optimizing the addition amount of sodium oxide, aluminum oxide, silicon oxide, zinc oxide, lead oxide, boron oxide and lithium oxide in the glass powder system, and with the cooperation of oxide regulators such as tellurium oxide, selenium oxide and tungsten oxide, the provided glass powder has appropriate etching ability and high-temperature melting characteristics, and has moderate etching ability for the passivation layer of the battery cell, reducing the recombination caused by the sintering of silver paste on the battery surface, ensuring that under the condition of the lower sintering temperature (690-730°C) of the LECO sintering technology, the silver electrode can still form a good ohmic contact with the high-square-resistance battery silicon substrate while maintaining a higher open circuit voltage, thereby effectively improving the photoelectric conversion efficiency of the TOPCon battery.

[0033] 3. The present invention adopts a platinum crucible for high-temperature smelting, thereby effectively avoiding the adverse effects of impurities in the crucible on the glass during the smelting process. The present invention further optimizes the screening after grinding with a planetary ball mill. After screening, a secondary grinding treatment is performed with a jet mill to obtain glass powder with a D50 particle size of 1.8 to 2 μm, so that the powder maintains a good glass structure, thereby ensuring the stability of subsequent applications.

[0034] 4. Compared with the traditional silver-aluminum paste glass powder used on the front side of N-type TOPCon, the glass powder provided by the present invention has a lower addition amount in the conductive silver paste and can meet the requirements of low contact resistance, high open circuit voltage and high photoelectric conversion efficiency on high square resistance TOPCon batteries, which greatly reduces the amount of glass powder used and truly removes metal aluminum, reduces unnecessary metal composites, and promotes the improvement of battery efficiency. DETAILED DESCRIPTION

[0035] Examples 1-4

[0036] Embodiments 1-4 of the present invention provide a glass powder for high square resistance TOPCon battery fine grid silver paste, and the formula is shown in Table 1 in terms of mass percentage.

[0037] Table 1

[0038]

[0039] On the other hand, embodiments 1-4 of the present invention provide a method for preparing glass powder for high square resistance TOPCon battery fine grid silver paste, comprising the following steps: placing sodium oxide, aluminum oxide, silicon oxide, zinc oxide, lead oxide, boron oxide, lithium oxide, and oxide regulator in a mixer, transferring them to a platinum crucible after mixing, placing the crucible in a sintering furnace at 1100°C, and smelting at high temperature for 30 minutes, then taking the crucible out of the sintering furnace and placing the melt in the crucible in a cooling roller for cold rolling treatment, placing the product after cold rolling treatment in a ball mill for ball milling treatment, sieving the product after ball milling, and then performing secondary grinding treatment to obtain glass powder. The ball mill is a planetary ball mill. The mass ratio of the grinding ball to the product after cold rolling treatment in the ball milling treatment is 5:1. The ball milling speed of the ball milling treatment is 200rpm, and the ball milling time is 120min. The screening is specifically performed using a 200-mesh screen. The secondary grinding treatment is performed using an airflow mill, the pressure of the airflow mill is 1.0MPa, and the secondary grinding treatment time is 20min. The D50 particle size of the glass powder is 1.8-2 μm.

[0040] Application Examples 1-4

[0041] Application Examples 1-4 of the present invention provide a high square resistance TOPCon battery fine grid silver paste, and the formula is shown in Table 2 in parts by weight.

[0042] Table 2

[0043]

[0044] Calculated by mass percentage, the organic carrier includes: 2.5% of ethyl cellulose, 2% of acrylic resin, 60% of pineneol, 20% of diethylene glycol methyl ether, 14.5% of butyl carbitol acetate, and 1% of lecithin.

[0045] The method for preparing the high square resistance TOPCon battery fine grid silver paste is as follows: silver powder, glass powder, organic carrier and solvent are mixed to obtain the paste.

[0046] Application comparison example

[0047] The control example of the present invention is the silver aluminum paste DK71A specially used for N-type TOPcon batteries commercially available from Wuxi Dike Electronic Materials Co., Ltd.

[0048] Performance Testing

[0049] The silver paste provided in the application examples 1-4 and the application control examples was respectively printed on the front of the 182mm×182mm TOPCon cell by screen printing, and the silver paste was uniformly printed on the back. The application examples 1-4 were sintered at a peak temperature of 730°C using a sintering furnace and light injection was performed, and then passed through the LECO equipment for laser-assisted sintering (LECO technology) to obtain the cell 1-4. The application control examples were divided into two groups, one group using a traditional sintering method (resistance wire heating chain sintering furnace, the highest sintering temperature of the sintering furnace was 750°C) to obtain the cell 5, and the other group using the same sintering method as the application examples 1-4 to obtain the cell 6. The photoelectric conversion efficiency (Eff), open circuit voltage (Uoc), short circuit current (Isc), fill factor (FF), series resistance (Rser), and parallel resistance (Rsh) of the cell 1-6 were tested by current-voltage performance. The test results are shown in Table 3.

[0050] Table 3

[0051] serial number Eff / % Uoc / V Isc / A FF / % Rser / Ω Rsh / Ω Battery Cell 1 25.656 0.7317 13.5806 85.01 0.00168 1909.4730 Battery Cell 2 25.746 0.7334 13.5820 85.14 0.00169 1945.5203 Battery Cell 3 25.874 0.7349 13.6033 85.44 0.00140 1989.3486 Battery Cell 4 25.761 0.7339 13.5980 85.21 0.00157 1960.0031 Battery Cell 5 25.484 0.7177 13.5811 84.99 0.00177 1938.0101 Battery Cell 6 25.491 0.7189 13.5847 85.02 0.00173 1996.7668

[0052] By analyzing the above table, it can be seen that the control example is sintered by traditional high-temperature sintering and LECO technology respectively, and there is no obvious difference in efficiency. However, compared with cell 5, cell 6 sintered by LECO technology has an extremely small advantage in open circuit voltage. Cells 1-4 are higher in efficiency than the control example, and have obvious advantages in open circuit voltage and filling factor parameters, which shows that traditional silver-aluminum paste cannot meet the process requirements of LECO sintering technology and the glass powder of the present invention can be better adapted. At the same time, the embodiment of the present invention adds oxide regulators, tellurium oxide, tungsten oxide, and selenium oxide to further adjust the fluidity of the glass during high-temperature sintering and the etching ability of the cell passivation layer, which are very helpful for the effective realization of LECO sintering. And the series resistance of the control example is high, which shows that the contact effect of traditional silver-aluminum paste on high-resistance batteries is also inferior to that of the embodiment of the present invention.

Claims

1. A glass powder for high square resistance TOPCon battery fine grid silver paste, It is characterized in that The raw materials for its preparation include at least, by weight: 1-10 parts of sodium oxide, 2-15 parts of aluminum oxide, 3-25 parts of silicon oxide, 5-15 parts of zinc oxide, 65-85 parts of lead oxide, 5-20 parts of boron oxide, 1-5 parts of lithium oxide, and 1-10 parts of an oxide regulator.

2. The glass powder for high square resistance TOPCon battery fine grid silver paste according to claim 1, It is characterized in that The oxide regulator is selected from at least one of tellurium oxide, selenium oxide, barium oxide, tungsten oxide and calcium oxide.

3. A method for preparing glass powder for high square resistance TOPCon battery fine grid silver paste according to any one of claims 1-2, It is characterized in that The method comprises at least the following steps: placing sodium oxide, aluminum oxide, silicon oxide, zinc oxide, lead oxide, boron oxide, lithium oxide and an oxide regulator in a mixer, transferring the mixture to a platinum crucible after mixing, placing the crucible in a sintering furnace at 1000-1100° C., and smelting at high temperature for 20-40 minutes, then taking the crucible out of the sintering furnace and placing the melt in the crucible on a cooling roller for cold rolling treatment, placing the product after the cold rolling treatment in a ball mill for ball milling treatment, sieving the product after ball milling, and then performing secondary grinding treatment to obtain glass powder.

4. The method for preparing glass powder for high square resistance TOPCon battery fine grid silver paste according to claim 3, It is characterized in that The D50 particle size of the glass powder is 1.8-2 μm.

5. The method for preparing glass powder for high square resistance TOPCon battery fine grid silver paste according to claim 3, It is characterized in that The mass ratio of the grinding balls in the ball milling process to the product after the cold rolling process is (3-6):

1.

6. The method for preparing glass powder for high square resistance TOPCon battery fine grid silver paste according to claim 3, It is characterized in that The ball milling speed of the ball milling treatment is 150-300 rpm, and the ball milling time is 90-180 min.

7. The method for preparing glass powder for high square resistance TOPCon battery fine grid silver paste according to claim 3, It is characterized in that The secondary grinding process is performed by using a jet mill, the pressure of the jet mill is 0.8-1.2 MPa, and the secondary grinding process time is 10-30 min.

8. Application of the glass powder for high square resistance TOPCon battery fine grid silver paste according to any one of claims 1-2, It is characterized in that The invention is applied to the preparation of fine grid silver paste of high square resistance TOPCon battery, wherein the addition amount of glass powder in the fine grid silver paste of high square resistance TOPCon battery is 1.5-3.0wt%.

9. Application of the glass powder for high square resistance TOPCon battery fine grid silver paste according to claim 8, It is characterized in that The raw materials for preparing the high square resistance TOPCon battery fine grid silver paste at least include glass powder, silver powder, organic carrier and organic solvent.

10. Application of the glass powder for high square resistance TOPCon battery fine grid silver paste according to claim 8, It is characterized in that The mass ratio of the silver powder, glass powder, organic carrier and solvent is (88-90):(1.5-3.0):(6-10):(2-5).

Citation Information

Patent Citations

  • Glass powder, preparation method thereof and application of glass powder in TOPCon battery

    CN112592068A

  • Glass powder suitable for crystalline silicon p + layer contact and used for thick film silver paste and preparation method of glass powder

    CN114380507A

  • Glass powder for TOPCON N-type crystalline silicon solar cell front silver paste and preparation method thereof

    CN114524618A

  • High-stability glass powder, preparation method thereof and application of high-stability glass powder in front fine grid silver paste of TOPCON battery

    CN116239307A

  • Glass powder for preparing solar cell electrode, paste composition comprising same, solar cell electrode, and solar cell

    WO2019056418A1