Artificial aggregate as well as preparation method and application thereof
By using the fine sand of concrete residue as the aggregate skeleton and covering the concrete waste residue-cement encapsulated leather, combined with specific adhesives and activaters, the problem of low compressive strength of waste residue in the concrete production process is solved, and efficient resource recovery is achieved and environmental protection.
Patent Information
- Application Number
- CN202410954600.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the pollution and resource waste generated during concrete production process, especially the low compressive strength of concrete waste slag cannot meet the use requirements, resulting in resource waste and environmental pollution.
The skeleton structure of concrete residue fine sand is used as the aggregate, and the concrete waste residue-cement encapsulated leather is coated with quaternized chitosan and alginate as the binder, titanium dioxide, gypsum and water glass are used as the exciter. Improve the compressive strength of the aggregate.
It significantly improves the compressive strength of artificial aggregates to 2.0~3.0MPa, has excellent mechanical properties, and promotes the recycling of concrete waste and efficient utilization of resources, reducing resource waste and environmental pollution.
Smart Images

Figure CN118908609A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete, and in particular relates to an artificial aggregate and a preparation method and application thereof. Background Art
[0002] At present, the annual consumption of concrete exceeds 4 billion cubic meters, and the consumption of sand and gravel aggregate exceeds 6 to 8 billion tons. Such a huge demand for sand and gravel aggregate has led to a large amount of mountain quarrying, which damages the ecological environment. Along with the huge output of concrete, the consumption of resources and energy has soared, and the pollution formed is also increasing. There are many pollutions generated when commercial concrete mixing stations produce concrete, mainly dust pollution in the air, water pollution when cleaning equipment, sound pollution generated by mixing stations during production, and residual concrete waste. In the prior art, most of the solid waste produced is usually directly discharged and landfilled or directly used to prepare fine stone aggregate using pure concrete waste. The discharge and landfill not only causes a waste of resources, but also occupies land and has the problem of environmental pollution; and the fine stone aggregate directly prepared using pure concrete waste has a low compressive strength (0.4 to 0.6 MPa) and cannot meet the use requirements. Summary of the invention
[0003] The object of the present invention is to provide an artificial aggregate and a preparation method and application thereof. The artificial aggregate provided by the present invention uses concrete residue fine sand as the skeleton structure of the aggregate and has excellent compressive strength.
[0004] In order to achieve the purpose of the present invention, the present invention provides the following technical solutions:
[0005] An artificial aggregate, comprising a concrete residue fine sand inner core and a concrete waste residue-cement encapsulating skin material coated on the surface of the concrete residue fine sand inner core;
[0006] The artificial aggregate includes the following raw materials by mass fraction:
[0007] Concrete residue powder 10-15%, cement 10-15%, concrete residue fine sand 40-45%, adhesive 5-10%, activator 5-10% and water 20-25%.
[0008] Preferably, the adhesive comprises quaternized chitosan and alginate; the mass ratio of the quaternized chitosan to alginate is 5-10:5-10.
[0009] Preferably, the activator comprises titanium dioxide, gypsum and water glass; the mass ratio of titanium dioxide, gypsum and water glass is 1-3:5-7:1-1.5.
[0010] Preferably, the concrete residue powder comprises hydrated cement and unhydrated cement; the mass ratio of the hydrated cement to the unhydrated cement is 3-6:1-3.
[0011] Preferably, the particle size of the concrete residue fine sand is 0.5-2 mm.
[0012] Preferably, the particle size of the inner core of the concrete residue fine sand is 4 to 10 mm; and the thickness of the concrete waste residue-cement packaging material is 1 to 5 mm.
[0013] The present invention also provides a method for preparing the artificial aggregate described in the above technical solution, comprising the following steps:
[0014] Mixing concrete residue fine sand, a binder and a portion of water, and performing a first granulation to obtain a concrete residue fine sand core;
[0015] The concrete residue fine sand core, concrete residue powder, cement, activator and remaining water are mixed and subjected to a second granulation to obtain the artificial aggregate.
[0016] Preferably, the rotation speeds of the first granulation and the second granulation are independently 40-60 r / min.
[0017] The present invention also provides the use of the artificial aggregate described in the above technical solution or the artificial aggregate prepared by the preparation method described in the above technical solution in concrete.
[0018] Preferably, the mass of the artificial aggregate in the concrete accounts for 20-30% of the total mass of the concrete.
[0019] The present invention provides an artificial aggregate, comprising a concrete residue fine sand inner core and a concrete waste slag-cement encapsulation skin coated on the surface of the concrete residue fine sand inner core; the artificial aggregate comprises the following preparation raw materials by mass fraction: 10-15% concrete residue powder, 10-15% cement, 40-45% concrete residue fine sand, 5-10% adhesive, 5-10% activator and 20-25% water. The present invention uses fine sand in concrete residue as the main skeleton structure of aggregate, so that waste is directly converted into the main component of the product, promotes the consumption of concrete waste, reduces the waste of resources, and the compressive strength of the artificial aggregate provided by the present invention can be significantly enhanced compared with the aggregate prepared by pure concrete waste; at the same time, the present invention adds an activator to the concrete residue powder, which can stimulate the activity of the concrete residue powder, and further improve the compressive strength of the enhanced artificial aggregate. It can be seen from the results of the embodiments of the present invention that the compressive strength of the artificial aggregate provided by the present invention is 2.0-3.0MPa, and the mechanical properties are excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0021] Figure 1 This is a physical picture of the concrete residue fine sand;
[0022] Figure 2 Figure 1 is a diagram of the preparation process of the regenerated sand aggregate core;
[0023] Figure 3 The line graph is the relationship between the compressive strength of different ratios of binder and artificial aggregate. DETAILED DESCRIPTION
[0024] The present invention provides an artificial aggregate, comprising a concrete residue fine sand inner core and a concrete waste residue-cement encapsulating skin material coated on the surface of the concrete residue fine sand inner core;
[0025] The artificial aggregate includes the following raw materials by mass fraction:
[0026] Concrete residue powder 10-15%, cement 10-15%, concrete residue fine sand 40-45%, adhesive 5-10%, activator 5-10% and water 20-25%.
[0027] In the present invention, unless otherwise specified, all preparation raw materials are preferably commercially available products well known to those skilled in the art.
[0028] In the present invention, the raw materials for preparing the artificial aggregate include 10-15% concrete residue powder, preferably 11-13% by mass fraction. In the present invention, the concrete residue powder preferably includes hydrated and unhydrated cement; the mass ratio of the hydrated and unhydrated cement is preferably 3-6:1-3, more preferably 3:1. In the present invention, the concrete residue powder serves as the main skeleton structure of the aggregate, wraps around the surface of the fine sand, and fills the tiny pores between the fine sand.
[0029] In the present invention, the raw materials for preparing the artificial aggregate include 10-15% cement, preferably 11-12% by mass. In the present invention, the cement is preferably silicate cement. In the present invention, the hydration reaction of cement is used to improve the gelling property of concrete waste residue, and the internal part of the aggregate is made denser through inorganic chemical reaction on the basis of the bio-adhesive, thereby improving the compressive strength of the aggregate.
[0030] In the present invention, the raw materials for preparing the artificial aggregate include 40-45% concrete residue fine sand, preferably 42-44% by mass fraction. In the present invention, the particle size of the concrete residue fine sand is preferably 0.5-2 mm, more preferably 1-1.5 mm. In the present invention, the concrete residue fine sand is preferably recovered from the concrete residue produced by the tank truck and the mixing equipment through the mud circulation recovery device of the commercial concrete mixing station, and then filtered, dried and screened in sequence. In the present invention, the screening is preferably performed by vibrating screen screening. In the present invention, the concrete residue fine sand plays a supporting role as the inner core skeleton of the aggregate.
[0031] In the present invention, the raw materials for preparing the artificial aggregate include 5-10% of a binder, preferably 6-8% by mass. In the present invention, the binder preferably includes quaternized chitosan (HACC) and alginate (SA). In the present invention, the alginate is preferably sodium alginate. In the present invention, the binder has the function of solidifying waste materials and improving the compressive strength of aggregates.
[0032] In the present invention, the mass ratio of the quaternized chitosan to alginate is preferably 5-10:5-10, more preferably 8-9:6-7.
[0033] In the present invention, the raw materials for preparing the artificial aggregate include 5-10% of the activator, preferably 6-8% by mass fraction. In the present invention, the activator preferably includes titanium dioxide, gypsum and water glass. In the present invention, the mass ratio of titanium dioxide, gypsum and water glass is preferably 1-3:5-7:1-1.5, more preferably 2:7:1. In the present invention, the activator has the function of solidifying the waste and improving the compressive strength of the aggregate.
[0034] In the present invention, the raw materials for preparing the artificial aggregate include 20-25% water, preferably 22-23% water, by mass fraction.
[0035] In the present invention, the artificial aggregate comprises a concrete residue fine sand core and a concrete waste slag-cement encapsulating skin material coated on the surface of the concrete residue fine sand core. In the present invention, the particle size of the concrete residue fine sand core is preferably 4 to 10 mm, more preferably 5 to 8 mm; the thickness of the concrete waste slag-cement encapsulating skin material is preferably 1 to 5 mm, more preferably 1.5 to 2.5 mm, and further preferably 2 mm.
[0036] In the present invention, the compressive strength of the artificial aggregate is preferably 2.0 to 3.0 MPa, more preferably 2.2 to 2.5 MPa.
[0037] The present invention also provides a method for preparing the artificial aggregate described in the above technical solution, comprising the following steps:
[0038] Mixing concrete residue fine sand, a binder and a portion of water, and performing a first granulation to obtain a concrete residue fine sand core;
[0039] The concrete residue fine sand core, concrete residue powder, cement, activator and remaining water are mixed and subjected to a second granulation to obtain the artificial aggregate.
[0040] The present invention mixes concrete residue fine sand, a binder and part of water, and performs a first granulation to obtain a concrete residue fine sand core. The present invention has no particular limitation on the mixing method and conditions, and the mixing method and conditions well known to those skilled in the art can be used.
[0041] In the present invention, curing is preferably performed after the first granulation. In the present invention, the curing temperature is preferably 20-25°C, more preferably 22°C; the relative humidity is preferably 90-95%, more preferably 92-93%; and the curing time is preferably 7-14 days, more preferably 10-12 days.
[0042] After obtaining the concrete residue fine sand kernel, the present invention mixes the concrete residue fine sand kernel, concrete residue powder, cement, activator and remaining water, and performs a second granulation to obtain the artificial aggregate. In the present invention, preferably, the concrete residue powder and cement are first mixed to obtain a mixed dry material; water glass and remaining water are second mixed to obtain a water glass solution; the concrete residue fine sand kernel, mixed dry material, titanium dioxide and gypsum are third mixed to perform a second granulation; the water glass solution is sprayed into the second granulation process to obtain the artificial aggregate. In the present invention, the mass ratio of the partial water to the remaining water is preferably 40-45:155-160, more preferably 42-43:157-158, and further preferably 42.5:157.5. The present invention does not specifically limit the manner and conditions of the first mixing, the second mixing and the third mixing, and the mixing manner and conditions well known to those skilled in the art can be used.
[0043] In the present invention, the first granulation and the second granulation are preferably carried out in a water chestnut-type coating machine; the rotation speeds of the first granulation and the second granulation are independently preferably 40 to 60 r / min.
[0044] In the present invention, curing is preferably performed after the second granulation, and the curing is preferably the same as the above-mentioned curing, which will not be described in detail here.
[0045] The present invention also provides the use of the artificial aggregate described in the above technical solution or the artificial aggregate prepared by the preparation method described in the above technical solution in concrete.
[0046] In the present invention, the mass of the artificial aggregate in the concrete preferably accounts for 20-30% of the total mass of the concrete, and more preferably 25-28wt%.
[0047] In order to further illustrate the present invention, the artificial aggregate provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0048] Example 1
[0049] 100 g of concrete residue fine sand (particle size of 0.5-2 mm) and 25 g of the binder solution of the proportion described in Table 1 were mixed, placed in a water chestnut-type coating machine (rotation speed 40 r / min) for the first granulation, and then cured for 7 days at 20° C. and 95% relative humidity to obtain the concrete residue fine sand inner core.
[0050] The compressive strength of the concrete residue fine sand core prepared in Example 1 was tested according to the single aggregate compressive bearing capacity test. The test results are shown in Tables 1 and Figure 1 shown.
[0051] Table 1 Test results of compressive strength of the binder ratio and concrete residue fine sand kernel in Example 1
[0052]
[0053] Figure 3 The relationship between the compressive strength of the binder and the concrete residue fine sand core with different ratios is shown in Table 1 and Figure 3 The results show that the best ratio of adhesive is HACC-9 / SA-6, that is, 9% chitosan ammonium salt and 6% sodium alginate.
[0054] Figure 1 This is a physical picture of fine sand from concrete residue.
[0055] Figure 2 Diagram of the preparation process of the recycled sand aggregate core.
[0056] Example 2
[0057] After mixing concrete residue fine sand, binder (HACC-8 / SA-7) and 42.5 g of water according to the proportions described in Table 2, the mixture was placed in a water chestnut-type coating machine (rotation speed 40 r / min) for the first granulation, and then cured for 7 days at 22° C. and 92% relative humidity to obtain a concrete residue fine sand core;
[0058] The concrete residue powder and silicate cement are mixed to obtain a mixed dry material; 5 g of water glass and 147.5 g of water are mixed to obtain a water glass solution;
[0059] The concrete residue fine sand core is soaked (10g water), mixed with the mixed dry material, 10g titanium dioxide and 35g gypsum, and then placed in a water chestnut-type coating machine for the second granulation. At the same time, the water glass solution is slowly sprayed into the second granulation process, and then cured for 7 days at 22°C and 92% relative humidity to obtain artificial aggregate.
[0060] According to the single aggregate compressive bearing capacity test on the artificial aggregate prepared in Example 2, the test results are shown in Table 2.
[0061] Table 2 Proportion of artificial aggregate and test results of artificial aggregate performance described in Example 2
[0062]
[0063] In Table 2, Group 1 is a control group test. Group 2 and Group 1 explore the effect of concrete waste shell with activator on the strength of artificial aggregate without cement and activator; Group 1 and Group 3 compare and explore the effect of concrete waste shell-cement-activator shell on the performance of artificial aggregate with cement. The results in Table 2 show the optimal composition of concrete waste shell-cement-activator in the artificial aggregate of the present invention.
[0064] Comparative Example 1
[0065] The concrete residue was placed in a granulator. According to the water-cement ratio of the concrete residue and water being 0.46, water was sprayed into the granulator in the form of mist using a spray bottle. Aggregates with a particle size of 4 to 10 mm were prepared at a rotation speed of 40 r / min. The aggregates were then allowed to stand for 6 hours and placed in a standard curing room for 7 days. The single aggregate compressive bearing capacity of the aggregate was tested to be 0.41 MPa.
[0066] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. An artificial aggregate, characterized in that: It comprises a concrete residue fine sand inner core and a concrete waste residue-cement encapsulating skin material coated on the surface of the concrete residue fine sand inner core; The artificial aggregate includes the following raw materials by mass fraction: Concrete residue powder 10-15%, cement 10-15%, concrete residue fine sand 40-45%, adhesive 5-10%, activator 5-10% and water 20-25%.
2. The artificial aggregate according to claim 1, characterized in that: The adhesive comprises quaternized chitosan and alginate; the mass ratio of the quaternized chitosan to the alginate is 5-10:5-10.
3. The artificial aggregate according to claim 1, characterized in that: The activator comprises titanium dioxide, gypsum and water glass; the mass ratio of the titanium dioxide, gypsum and water glass is 1-3:5-7:1-1.
5.
4. The artificial aggregate according to claim 1, characterized in that: The concrete residue powder includes hydrated cement and unhydrated cement; the mass ratio of the hydrated cement to the unhydrated cement is 3-6:1-3.
5. The artificial aggregate according to claim 1, characterized in that: The particle size of the concrete residue fine sand is 0.5-2 mm.
6. The artificial aggregate according to claim 1, characterized in that: The particle size of the concrete residue fine sand inner core is 4-10 mm; the thickness of the concrete waste residue-cement packaging skin material is 1-5 mm.
7. The method for preparing the artificial aggregate according to any one of claims 1 to 6, characterized in that: The following steps are involved: Mixing concrete residue fine sand, a binder and a portion of water, and performing a first granulation to obtain a concrete residue fine sand core; The concrete residue fine sand core, concrete residue powder, cement, activator and remaining water are mixed and subjected to a second granulation to obtain the artificial aggregate.
8. The preparation method according to claim 7, characterized in that: The rotation speeds of the first granulation and the second granulation are independently 40 to 60 r / min.
9. Use of the artificial aggregate according to any one of claims 1 to 6 or the artificial aggregate prepared by the preparation method according to claim 7 or 8 in concrete.