Superfine powder-containing concrete for pipe pile and preparation method thereof

By using counterion quaternary ammonium salt and carbon fiber in concrete, a conductive network is formed, which solves the problem of insufficient corrosion resistance of prestressed high-strength concrete in complex environments, and achieves high strength, permeability and compressive strength Improvement, suitable for foundation structures in coastal and industrially polluted areas.

CN118908638APending Publication Date: 2024-11-08ANHUI DONGCAI MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411145514.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing prestressed high-strength concrete has limited corrosion resistance in coastal areas, industrial polluted areas and complex geological environments, which limits its application scope.

Method used

Using counterion quaternary ammonium salt as an admixture, the quaternary ammonium cations generated by reacting with methyl carbonate quaternary ammonium salt and carboxylic acid form a dense adsorption film, which improves the antibacterial and corrosion resistance of concrete, and interlocks with carbon fibers. The conductive network optimizes the internal structure of concrete.

Benefits of technology

It significantly improves the corrosion resistance and mechanical properties of concrete, improves compressive strength and permeability, and gives concrete excellent comprehensive performance, suitable for building infrastructure in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005002087200000111
    Figure BDA0005002087200000111
  • Figure BDA0005002087200000121
    Figure BDA0005002087200000121
Patent Text Reader

Abstract

The invention relates to the field of building materials (IPC classification number: C04B), in particular to superfine powder-containing concrete for a tubular pile and a preparation method of the superfine powder-containing concrete. The concrete for the pipe pile is prepared from the following raw materials in parts by weight: 190 to 500 parts of cement, 550 to 1400 parts of coarse aggregate, 300 to 800 parts of fine aggregate, 40 to 110 parts of superfine powder, 20 to 50 parts of additive, 12 to 35 parts of carbon fiber, 2 to 9 parts of water reducing agent and 70 to 180 parts of solvent. By compounding the raw materials and particularly adding the self-made admixture, the concrete for the pipe pile, which is high in strength, good in anti-permeability effect and excellent in corrosion resistance, is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building materials (IPC classification number: C04B), and in particular to ultrafine powder-containing concrete for pipe piles and a preparation method thereof. Background Art

[0002] Prestressed high-strength concrete piles are a commercial prefabricated concrete component with the advantages of high strength, good durability, convenient construction, and short production cycle. They are mostly used as the foundation structure of buildings. The traditional preparation process of prestressed high-strength concrete is a combination of normal pressure steam curing and high pressure steam curing, which not only causes a large energy consumption, but also has environmental pollution problems.

[0003] In recent years, technicians in this field have obtained autoclave-free high-strength concrete pipe piles by improving raw materials and adding admixtures. However, with the promotion of prestressed high-strength concrete applications, the market has put forward higher requirements for prestressed high-strength concrete, especially requiring concrete to have high strength, impermeability, and corrosion resistance.

[0004] In response to this requirement, Chinese patent CN116177967B discloses a method for preparing high-strength concrete, which adds organic nano hollow spheres and modified calcium sulfate whiskers to avoid the problems of rapid slump loss and water seepage of high-strength concrete, and effectively improves the compressive strength, durability and low-temperature resistance of concrete. Chinese patent CN108623265B discloses a high-strength impermeable concrete and its production method, which adjusts the fluidity, intrinsic hydration effect and expansion effect of concrete after solidification by adding a fine powder composition composed of silicon micropowder, polyetheretherketone and alumina, a tensile composition, magnesium oxide and an air entraining agent to obtain high-strength concrete with good impermeability effect. However, the above-mentioned prior art does not pay attention to the corrosion resistance of high-strength concrete. The corrosion resistance of concrete is limited, which limits its application in coastal areas, industrial pollution areas and complex geological environments.

[0005] In this context, how to improve the corrosion resistance and enhance the comprehensive performance of concrete while maintaining its high strength has become a technical problem that needs to be urgently solved in this field. Summary of the invention

[0006] The invention provides concrete for pipe piles containing special ultrafine powder and a preparation method thereof. By compounding raw materials, especially adding homemade admixtures, concrete for pipe piles with high strength, good anti-seepage effect and excellent corrosion resistance is obtained.

[0007] The first aspect of the present invention provides a concrete for pipe piles containing ultrafine powder. The raw materials for preparing the concrete for pipe piles include, by weight, 190-500 parts of cement, 550-1400 parts of coarse aggregate, 300-800 parts of fine aggregate, 40-110 parts of ultrafine powder, 20-50 parts of admixture, 12-35 parts of carbon fiber, 2-9 parts of water reducer, and 70-180 parts of water.

[0008] In some preferred embodiments, the admixture is a counter ion quaternary ammonium salt.

[0009] In some preferred embodiments, the admixture accounts for 2-15 wt % of the total amount of the gel material, and the gel material consists of cement and ultrafine powder.

[0010] Preferably, the additive accounts for 3-12 wt % of the total amount of the gel material.

[0011] Further preferably, the additive accounts for 5-10 wt % of the total amount of the gel material.

[0012] In some preferred embodiments, the water reducing agent accounts for 0.1-2 wt % of the total amount of the gel material.

[0013] Preferably, the water reducing agent accounts for 0.2-0.5 wt % of the total amount of the gel material.

[0014] In some preferred embodiments, the raw materials for preparing the counter ion quaternary ammonium salt include methyl carbonate quaternary ammonium salt and carboxylic acid.

[0015] In some preferred embodiments, the mass ratio of methyl carbonate quaternary ammonium salt to carboxylic acid is 1:(0.1-0.5).

[0016] Preferably, the mass ratio of methyl carbonate quaternary ammonium salt to carboxylic acid is 1:(0.20-0.35).

[0017] In some preferred embodiments, the raw materials for preparing the methyl carbonate quaternary ammonium salt include dialkylmethyl tertiary amine and dimethyl carbonate.

[0018] In some preferred embodiments, the dialkylmethyl tertiary amine includes C5-C 20 Dialkylmethyl tertiary amine.

[0019] Preferably, the dialkylmethyl tertiary amine is C 10 -C 16 Dialkylmethyl tertiary amine.

[0020] Examples of the dialkylmethyl tertiary amine include at least one of dioctylmethyl tertiary amine, didecylmethyl tertiary amine, didodecylmethyl tertiary amine, ditetradecylmethyl tertiary amine, and dihexadecylmethyl tertiary amine.

[0021] In some preferred embodiments, the molar ratio of dialkylmethyl tertiary amine to dimethyl carbonate is 1:

[0022] (1-10).

[0023] Preferably, the molar ratio of dialkylmethyl tertiary amine to dimethyl carbonate is 1:(2-7).

[0024] In some preferred embodiments, the preparation method of methyl carbonate quaternary ammonium salt comprises: mixing dialkyl methyl tertiary amine, dimethyl carbonate and solvent, reacting at 90-165° C. and 0.3-2 MPa for 0.5-7 h, and drying the reaction product at 75-85° C. for 12-20 h to obtain a methyl carbonate quaternary ammonium salt product.

[0025] Preferably, the preparation method of methyl carbonate quaternary ammonium salt comprises: mixing dialkyl methyl tertiary amine, dimethyl carbonate and solvent, reacting at 100-150° C. and 0.5-1.5 MPa for 1-5 hours, and drying the reaction product at 77-82° C. for 14-18 hours to obtain methyl carbonate quaternary ammonium salt product.

[0026] In some preferred embodiments, the solvent is selected from alcohol solvents, and the alcohol solvents are commonly used alcohol solvents in the art without particular limitation; for example, methanol, ethanol, isopropanol, glycerol, butanol, and the like.

[0027] In some preferred embodiments, the chain length of the carboxylic acid is C2-C 18 .

[0028] Preferably, the chain length of the carboxylic acid is C3-C 12 .

[0029] More preferably, the chain length of the carboxylic acid is C6-C 10 .

[0030] In some preferred embodiments, the carboxylic acid is at least one of hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, and decanoic acid.

[0031] In some preferred embodiments, the preparation method of the admixture is: adding methyl carbonate quaternary ammonium salt to a solvent, stirring continuously at 20-75° C., after the methyl carbonate quaternary ammonium salt is completely dissolved, adding carboxylic acid while stirring, stirring for 10-240 minutes; then recrystallizing, drying to constant weight, and obtaining an admixture product.

[0032] Preferably, the preparation method of the admixture is: adding methyl carbonate quaternary ammonium salt to a solvent, stirring continuously at 30-70° C., adding carboxylic acid while stirring after the methyl carbonate quaternary ammonium salt is completely dissolved, and stirring for 20-200 minutes; then recrystallizing, and drying at 50-80° C. to constant weight to obtain an admixture product.

[0033] In some preferred embodiments, the solvent is an alcohol solvent, and the alcohol solvent is a commonly used alcohol solvent in the art without particular limitation; for example, methanol, ethanol, isopropanol, glycerol, butanol, and the like.

[0034] Concrete pipe piles are often used as the foundation structure of buildings, which requires that their anti-seepage and anti-corrosion properties must be qualified, otherwise it will affect the stability of the foundation and even pose a greater risk. Quaternary ammonium salt compounds have antibacterial properties, but when they are used in concrete, they are limited by the complex use environment of concrete for pipe piles, and the corrosion resistance of conventional quaternary ammonium salt compounds is not significant.

[0035] The inventor unexpectedly discovered during the research that the use of counterion quaternary ammonium salt as an admixture can significantly improve the corrosion resistance of concrete; especially the use of C5-C 20 The methyl carbonate quaternary ammonium salt prepared from dialkylmethyl tertiary amine and dimethyl carbonate is further reacted with a C2-C 18 The carboxylic acid reacts to form a counterion quaternary ammonium salt. The quaternary ammonium cations in the admixture can be neatly arranged on the surface of the steel bar to form a dense adsorption film, thereby improving the antibacterial and corrosion inhibition effects of the concrete. At the same time, it is speculated that the tendency of the counterion end to generate insoluble organic carboxylate calcium in situ with the calcium ions in the system is enhanced, which optimizes the internal pore structure of the concrete, improves the material density, and improves the anti-permeability performance of the product.

[0036] Furthermore, the counterion quaternary ammonium salt reacts with the groups on the surface of the carbon fiber, improving the uniform dispersion of the carbon fiber in the concrete, constructing an interactively overlapped conductive network, synergistically exerting a cathodic protection effect, and improving the corrosion resistance and mechanical properties of concrete products. By compounding the counterion quaternary ammonium salt with ultrafine powder, carbon fiber and other raw materials, the antibacterial and corrosion resistance of the concrete can be improved, and the compressive strength and impermeability of the product can also be improved at the same time; giving the concrete products excellent comprehensive performance.

[0037] In some preferred embodiments, the ultrafine powder includes, by weight: 15-40 parts of slag, 10-30 parts of fly ash, 10-30 parts of slaked lime, and 5-10 parts of silica fume.

[0038] The average particle size of the slag is 1-50 μm; preferably, the average particle size of the slag is 2-35 μm.

[0039] The average particle size of the fly ash is 1-50 μm; preferably, the average particle size of the fly ash is 3-25 μm.

[0040] The average specific surface area of ​​slaked lime is 200-800m 2 / kg; preferably, the average specific surface area of ​​slaked lime is 300-600m 2 / kg.

[0041] The average specific surface area of ​​silica fume is 12000-40000m 2 / kg; preferably, the average specific surface area of ​​silica fume is 15000-35000m 2 / kg.

[0042] In some preferred embodiments, the carbon fibers have a length of 1-10 mm and a diameter of 5-15 μm.

[0043] Preferably, the carbon fiber has a length of 2-8 mm and a diameter of 7-12 μm.

[0044] In some preferred embodiments, the water reducer includes at least one of a naphthalene-based water reducer, a sulfonate-based water reducer, a polycarboxylic acid-based water reducer, and an amino-based water reducer.

[0045] Preferably, the water reducer includes a naphthalene-based water reducer and / or a polycarboxylic acid-based water reducer.

[0046] In some preferred embodiments, the average particle size of the coarse aggregate is 5-25 mm; preferably, the average particle size of the coarse aggregate is 6-18 mm.

[0047] In some preferred embodiments, the average particle size of the fine aggregate is 0.1-10 mm; preferably, the average particle size of the fine aggregate is 0.3-4 mm.

[0048] The second aspect of the present invention provides a method for preparing concrete for pipe piles containing ultrafine powder, and the preparation steps of the concrete for pipe piles include: 1) mixing cement, coarse aggregate, fine aggregate, ultrafine powder, carbon fiber, water reducer and water, and stirring evenly to obtain a mixture; 2) adding an admixture to the mixture prepared in step 1), stirring evenly to obtain concrete for pipe piles.

[0049] Beneficial effects:

[0050] The present invention provides a concrete for pipe piles containing ultrafine powder and a preparation method thereof, which has the following advantages:

[0051] (1) The present invention introduces counter-ion quaternary ammonium salt as an admixture into the concrete formula for pipe piles, and the quaternary ammonium cation forms a dense protective film on the surface of the steel bar, thereby improving the antibacterial and corrosion resistance of the concrete.

[0052] (2) The present invention selects methyl carbonate quaternary ammonium salts and carboxylic acids with suitable carbon chain lengths so that the admixtures can not only play a protective and corrosion-inhibiting role, but also the counter-ion end can react with calcium ions in the system in situ to generate insoluble substances, optimize the internal pore structure of concrete, improve the density of the material, and further improve the anti-seepage performance of the product.

[0053] (3) The structure and addition amount of the admixture are designed in the present invention so that it can also react with the groups on the surface of the carbon fiber, thereby improving the uniform dispersion of the carbon fiber in the concrete, constructing an interactively overlapped conductive network, synergistically exerting a cathodic protection effect, and further improving the corrosion resistance and mechanical properties of the product.

[0054] (4) The present invention selects a specific ultrafine powder formula, which works synergistically with admixtures, carbon fiber, etc., and uses cheap and readily available raw materials to prepare high-performance concrete, which has high economic value in the field of building materials.

[0055] (5) The present invention has simple process, safe and environmentally friendly operation, is easy to implement industrially, and has broad application prospects. DETAILED DESCRIPTION

[0056] Example

[0057] The ultrafine powder-containing concrete for pipe piles of the present invention comprises, by weight, 190-500 parts of cement, 550-1400 parts of coarse aggregate, 300-800 parts of fine aggregate, 40-110 parts of ultrafine powder, 20-50 parts of admixture, 12-35 parts of carbon fiber, 2-9 parts of water reducer and 70-180 parts of water.

[0058] A concrete for pipe piles containing ultrafine powder, comprising at least the following preparation steps:

[0059] 1) Mix cement, coarse aggregate, fine aggregate, ultrafine powder, carbon fiber, water reducing agent and water, and stir to obtain a mixture;

[0060] 2) Adding an admixture to the mixture prepared in step 1) and stirring evenly to obtain concrete for pipe piles.

[0061] In some embodiments, the admixture is a counterion quaternary ammonium salt.

[0062] In some embodiments, the additive accounts for 2-15 wt % of the total amount of the gel material, preferably 3-12 wt %. Further preferably, the additive accounts for 5-10 wt % of the total amount of the gel material.

[0063] In some embodiments, the gel material consists of cement and micronized powder.

[0064] In some embodiments, the water reducing agent accounts for 0.1-2 wt % of the total amount of the gel material.

[0065] In some embodiments, the water reducing agent accounts for 0.2-0.5 wt % of the total amount of the gel material.

[0066] In some embodiments, the raw materials for preparing the counter ion quaternary ammonium salt include methyl carbonate quaternary ammonium salt and carboxylic acid.

[0067] In some embodiments, the mass ratio of the methyl carbonate quaternary ammonium salt to the carboxylic acid is 1:(0.1-0.5).

[0068] In some embodiments, the mass ratio of the methyl carbonate quaternary ammonium salt to the carboxylic acid is 1:(0.20-0.35).

[0069] In some embodiments, the raw materials for preparing the methyl carbonate quaternary ammonium salt include dialkylmethyl tertiary amine and dimethyl carbonate.

[0070] In some embodiments, the dialkylmethyl tertiary amine includes C5-C 20 Dialkylmethyl tertiary amine.

[0071] In some embodiments, the dialkylmethyl tertiary amine is C 10 -C 16 Dialkylmethyl tertiary amine.

[0072] In some embodiments, the dialkylmethyl tertiary amine includes at least one of dioctylmethyl tertiary amine, didecylmethyl tertiary amine, didodecylmethyl tertiary amine, didetradecylmethyl tertiary amine, and didhexadecylmethyl tertiary amine.

[0073] In some embodiments, the molar ratio of dialkylmethyl tertiary amine to dimethyl carbonate is 1:(1-10).

[0074] In some embodiments, the molar ratio of dialkylmethyl tertiary amine to dimethyl carbonate is 1:(2-7).

[0075] In some embodiments, the preparation method of methyl carbonate quaternary ammonium salt includes: mixing dialkyl methyl tertiary amine, dimethyl carbonate and solvent, reacting at 90-165° C. and 0.3-2 MPa for 0.5-7 h, and drying the reaction product at 75-85° C. for 12-20 h to obtain a methyl carbonate quaternary ammonium salt product.

[0076] In some embodiments, the preparation method of methyl carbonate quaternary ammonium salt includes: mixing dialkyl methyl tertiary amine, dimethyl carbonate and solvent, reacting at 100-150° C. and 0.5-1.5 MPa for 1-5 hours, and drying the reaction product at 77-82° C. for 14-18 hours to obtain a methyl carbonate quaternary ammonium salt product.

[0077] In some embodiments, the solvent is selected from alcohol solvents, and the alcohol solvents are commonly used alcohol solvents in the art without particular limitation; for example, methanol, ethanol, isopropanol, glycerol, butanol, and the like.

[0078] In some embodiments, the chain length of the carboxylic acid is C2-C 18 .

[0079] In some embodiments, the chain length of the carboxylic acid is C3-C 12 .

[0080] In some embodiments, the chain length of the carboxylic acid is C6-C 10 .

[0081] In some embodiments, the carboxylic acid is at least one of hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, and decanoic acid.

[0082] In some embodiments, the preparation method of the admixture includes: adding methyl carbonate quaternary ammonium salt to a solvent, stirring continuously at 20-75° C., and after the methyl carbonate quaternary ammonium salt is completely dissolved, adding carboxylic acid while stirring, and stirring for 10-240 minutes; then recrystallizing, drying to constant weight, and obtaining an admixture product.

[0083] In some embodiments, the preparation method of the admixture includes: adding methyl carbonate quaternary ammonium salt to an alcohol solvent, stirring continuously at 30-70°C, and after the methyl carbonate quaternary ammonium salt is completely dissolved, adding carboxylic acid while stirring, and stirring for 20-200 minutes; then recrystallizing, and drying at 50-80°C to constant weight to obtain an admixture product.

[0084] In some embodiments, the solvent is an alcohol solvent, and the alcohol solvent is a commonly used alcohol solvent in the art without special limitation.

[0085] In some embodiments, the alcohol solvent is methanol, ethanol, isopropanol, glycerol, butanol, etc.

[0086] Concrete pipe piles are often used as the foundation structure of buildings, which requires that their anti-seepage and anti-corrosion properties must be qualified, otherwise it will affect the stability of the foundation and even pose a greater risk. Quaternary ammonium salt compounds have antibacterial properties, but when they are used in concrete, they are limited by the complex use environment of concrete for pipe piles, and the corrosion resistance of conventional quaternary ammonium salt compounds is not significant.

[0087] The inventor unexpectedly discovered during the research that the use of counterion quaternary ammonium salt as an admixture can significantly improve the corrosion resistance of concrete; especially the use of C5-C 20 The methyl carbonate quaternary ammonium salt prepared from dialkylmethyl tertiary amine and dimethyl carbonate is further reacted with a C2-C 18 The carboxylic acid reacts to form a counterion quaternary ammonium salt. The quaternary ammonium cations in the admixture can be neatly arranged on the surface of the steel bar to form a dense adsorption film, thereby improving the antibacterial and corrosion inhibition effects of the concrete. At the same time, it is speculated that the tendency of the counterion end to generate insoluble organic carboxylate calcium in situ with the calcium ions in the system is enhanced, which optimizes the internal pore structure of the concrete, improves the material density, and improves the anti-permeability performance of the product.

[0088] Furthermore, the counterion quaternary ammonium salt reacts with the groups on the surface of the carbon fiber, improving the uniform dispersion of the carbon fiber in the concrete, constructing an interactively overlapped conductive network, synergistically exerting a cathodic protection effect, and improving the corrosion resistance and mechanical properties of concrete products. By compounding the counterion quaternary ammonium salt with ultrafine powder, carbon fiber and other raw materials, the antibacterial and corrosion resistance of the concrete can be improved, and the compressive strength and impermeability of the product can also be improved at the same time; giving the concrete products excellent comprehensive performance.

[0089] In some embodiments, the ultrafine powder includes, by weight: 15-40 parts of slag, 10-30 parts of fly ash, 10-30 parts of slaked lime, and 5-10 parts of silica fume.

[0090] In some embodiments, the average particle size of the slag is 1-50 μm.

[0091] In some embodiments, the average particle size of the slag is 2-35 μm.

[0092] In some embodiments, the average particle size of the fly ash is 1-50 μm.

[0093] In some embodiments, the average particle size of the fly ash is 3-25 μm.

[0094] In some embodiments, the average specific surface area of ​​slaked lime is 200-800 m 2 / kg.

[0095] In some embodiments, the average specific surface area of ​​slaked lime is 300-600 m 2 / kg.

[0096] In some embodiments, the carbon fibers have a length of 1-10 mm and a diameter of 5-15 μm.

[0097] In some embodiments, the carbon fibers are 2-8 mm in length and 7-12 μm in diameter.

[0098] In some embodiments, the water reducer includes at least one of a naphthalene-based water reducer, a sulfonate-based water reducer, a polycarboxylic acid-based water reducer, and an amino-based water reducer.

[0099] In some embodiments, the water reducer includes a naphthalene-based water reducer and / or a polycarboxylic acid-based water reducer.

[0100] In some embodiments, the average particle size of the coarse aggregate is 5-25 mm.

[0101] In some embodiments, the average particle size of the coarse aggregate is 6-18 mm.

[0102] In some embodiments, the average particle size of the fine aggregate is 0.1-10 mm.

[0103] In some embodiments, the average particle size of the fine aggregate is 0.3-4 mm.

[0104] The concrete for pipe piles prepared according to the above scheme has higher strength, better permeability and excellent corrosion resistance.

[0105] Example 1

[0106] The first aspect of the present embodiment provides a concrete for pipe piles containing ultrafine powder. The raw materials for preparing the concrete for pipe piles include, by weight: 350 parts of cement, 980 parts of crushed stone (coarse aggregate, with an average particle size of 8 mm), 540 parts of river sand (fine aggregate, with an average particle size of 2 mm), 75 parts of ultrafine powder, 35 parts of admixture, 24 parts of carbon fiber, 5 parts of polycarboxylic acid water reducer, and 125 parts of water.

[0107] The admixture is a counterion quaternary ammonium salt, which is prepared by the following method:

[0108] (1) Preparation of methyl carbonate quaternary ammonium salt:

[0109] 26 parts of didodecylmethyl tertiary amine, 25.5 parts of dimethyl carbonate and 150 parts of ethanol were mixed, reacted at 125°C and 1MPa for 3 hours, and the reaction product was dried at 80°C for 16 hours to obtain a methyl carbonate quaternary ammonium salt product;

[0110] (2) Preparation of counterion quaternary ammonium salt:

[0111] 30 parts of methyl carbonate quaternary ammonium salt are added to 150 parts of ethanol, and stirred continuously at 50°C. After the methyl carbonate quaternary ammonium salt is completely dissolved, 8 parts of octanoic acid are added while stirring, and stirred for 150 minutes; recrystallized from ethyl acetate, dried at 60°C to constant weight, and a counterion quaternary ammonium salt product is obtained, wherein the mass ratio of methyl carbonate quaternary ammonium salt to octanoic acid is 1:0.27.

[0112] The ultrafine powder is uniformly mixed with 30 parts of slag, 19 parts of fly ash, 18 parts of slaked lime and 8 parts of silica fume.

[0113] The average particle size of slag is 25 μm, the average particle size of fly ash is 18 μm, and the average specific surface area of ​​slaked lime is 450 m 2 / kg, the average specific surface area of ​​silica fume is 25000m 2 / kg.

[0114] The length of the carbon fiber is 3-6 mm and the diameter is 8±0.5 μm.

[0115] The second aspect of the present embodiment provides a method for preparing concrete for pipe piles containing ultrafine powder, and the preparation steps of the concrete for pipe piles include: 1) mixing cement, coarse aggregate, fine aggregate, ultrafine powder, carbon fiber, water reducer, and water, and stirring evenly to obtain a mixture; 2) adding an admixture to the mixture prepared in step 1), stirring evenly, and obtaining concrete for pipe piles.

[0116] Example 2

[0117] The first aspect of the present embodiment provides a concrete for pipe piles containing ultrafine powder. The raw materials for preparing the concrete for pipe piles include, by weight: 195 parts of cement, 550 parts of crushed stone (coarse aggregate, with an average particle size of 10 mm), 300 parts of river sand (fine aggregate, with an average particle size of 4 mm), 40 parts of ultrafine powder, 20 parts of admixture, 12 parts of carbon fiber, 3 parts of polycarboxylic acid water reducer, and 70 parts of water.

[0118] The admixture is a counterion quaternary ammonium salt, which is prepared by the following method:

[0119] (1) Preparation of methyl carbonate quaternary ammonium salt:

[0120] 26 parts of didodecylmethyl tertiary amine, 25.5 parts of dimethyl carbonate and 150 parts of ethanol were mixed, reacted at 110°C and 1.5MPa for 4 hours, and the reaction product was dried at 77°C for 18 hours to obtain a methyl carbonate quaternary ammonium salt product;

[0121] (2) Preparation of counterion quaternary ammonium salt:

[0122] 20 parts of methyl carbonate quaternary ammonium salt are added to 150 parts of ethanol, and stirred continuously at 60°C. After the methyl carbonate quaternary ammonium salt is completely dissolved, 4 parts of octanoic acid are added while stirring, and stirred for 130 minutes; recrystallized from ethyl acetate, dried at 70°C to constant weight, and an admixture product is obtained, wherein the mass ratio of methyl carbonate quaternary ammonium salt to carboxylic acid is 1:0.2.

[0123] The ultrafine powder is uniformly mixed with 15 parts of slag, 10 parts of fly ash, 10 parts of slaked lime and 5 parts of silica fume.

[0124] The average particle size of slag is 23 μm, the average particle size of fly ash is 16 μm, and the average specific surface area of ​​slaked lime is 430 m 2 / kg, the average specific surface area of ​​silica fume is 27000m 2 / kg.

[0125] The carbon fiber has a length of 4-7 mm and a diameter of 7±0.5 μm.

[0126] The second aspect of the present embodiment provides a method for preparing concrete for pipe piles containing ultrafine powder, and the preparation steps of the concrete for pipe piles include: 1) mixing cement, coarse aggregate, fine aggregate, ultrafine powder, carbon fiber, water reducer, and water, and stirring evenly to obtain a mixture; 2) adding an admixture to the mixture prepared in step 1), stirring evenly, and obtaining concrete for pipe piles.

[0127] Example 3

[0128] The first aspect of the present embodiment provides a concrete for pipe piles containing ultrafine powder. The raw materials for preparing the concrete for pipe piles include, by weight: 500 parts of cement, 1400 parts of crushed stone (coarse aggregate, with an average particle size of 6 mm), 800 parts of river sand (fine aggregate, with an average particle size of 1 mm), 110 parts of ultrafine powder, 50 parts of admixture, 35 parts of carbon fiber, 9 parts of polycarboxylic acid water reducer, and 180 parts of water.

[0129] The admixture is a counterion quaternary ammonium salt, which is prepared by the following method:

[0130] (1) Preparation of methyl carbonate quaternary ammonium salt:

[0131] 26 parts of didodecylmethyl tertiary amine, 25.5 parts of dimethyl carbonate and 150 parts of ethanol were mixed, reacted at 140°C and 0.8MPa for 2 hours, and the reaction product was dried at 82°C for 15 hours to obtain a methyl carbonate quaternary ammonium salt product;

[0132] (2) Preparation of counterion quaternary ammonium salt:

[0133] 40 parts of methyl carbonate quaternary ammonium salt are added to 200 parts of ethanol, and the mixture is continuously stirred at 40°C. After the methyl carbonate quaternary ammonium salt is completely dissolved, 13 parts of octanoic acid are added while stirring, and the mixture is stirred for 170 minutes. The mixture is recrystallized from ethyl acetate and dried at 50°C to constant weight to obtain an admixture product, in which the mass ratio of methyl carbonate quaternary ammonium salt to octanoic acid is 1:0.33.

[0134] The ultrafine powder is uniformly mixed by 40 parts of slag, 30 parts of fly ash, 30 parts of slaked lime and 10 parts of silica fume.

[0135] The average particle size of slag is 27 μm, the average particle size of fly ash is 17 μm, and the average specific surface area of ​​slaked lime is 470 m 2 / kg, the average specific surface area of ​​silica fume is 30000m 2 / kg.

[0136] The length of the carbon fiber is 2-6 mm and the diameter is 9±0.5 μm.

[0137] The second aspect of the present embodiment provides a method for preparing concrete for pipe piles containing ultrafine powder, and the preparation steps of the concrete for pipe piles include: 1) mixing cement, coarse aggregate, fine aggregate, ultrafine powder, carbon fiber, water reducer, and water, and stirring evenly to obtain a mixture; 2) adding an admixture to the mixture prepared in step 1), stirring evenly, and obtaining concrete for pipe piles.

[0138] Example 4

[0139] This embodiment provides a concrete for pipe piles containing ultrafine powder and a preparation method thereof; the specific implementation method is the same as that of Example 1; the difference is that 34 parts of methyl carbonate quaternary ammonium salt are used to prepare the counter-ion quaternary ammonium salt, and 4 parts of octanoic acid are used, that is, the mass ratio of methyl carbonate quaternary ammonium salt to octanoic acid is 1:0.12.

[0140] Example 5

[0141] This embodiment provides a concrete for pipe piles containing ultrafine powder and a preparation method thereof; the specific implementation method is the same as that of Example 1; the difference is that 26 parts of methyl carbonate quaternary ammonium salt are used to prepare the counter-ion quaternary ammonium salt, and 12 parts of octanoic acid are used, that is, the mass ratio of methyl carbonate quaternary ammonium salt to octanoic acid is 1:0.46.

[0142] Comparative Example 1

[0143] This comparative example provides a concrete for pipe piles containing ultrafine powder and a preparation method thereof; the specific implementation method is the same as that of Example 1; the difference is that, in parts by weight, the raw materials for preparing the concrete for pipe piles include: 350 parts of cement, 998 parts of crushed stone (coarse aggregate, with an average particle size of 8 mm), 557 parts of river sand (fine aggregate, with an average particle size of 2 mm), 75 parts of ultrafine powder, 0 parts of admixture, 24 parts of carbon fiber, 5 parts of polycarboxylic acid water reducer, and 125 parts of water.

[0144] Comparative Example 2

[0145] This comparative example provides a concrete for pipe piles containing ultrafine powder and a preparation method thereof; the specific implementation method is the same as that of Example 1; the difference is that the admixture is the methyl carbonate quaternary ammonium salt described in Example 1; that is, octanoic acid is not introduced.

[0146] Comparative Example 3

[0147] This comparative example provides a concrete for pipe piles containing ultrafine powder and a preparation method thereof; the specific implementation method is the same as that of Example 1; the difference is that propionic acid is used instead of octanoic acid, that is, the carboxylic acid used to prepare the counter-ion quaternary ammonium salt is propionic acid.

[0148] Comparative Example 4

[0149] This comparative example provides a concrete for pipe piles containing ultrafine powder and a preparation method thereof; the specific implementation method is the same as that of Example 1; the difference is that myristic acid is used instead of caprylic acid, that is, the carboxylic acid used to prepare the counter-ion quaternary ammonium salt is myristic acid.

[0150] Comparative Example 5

[0151] This comparative example provides a concrete for pipe piles containing ultrafine powder and a preparation method thereof; the specific implementation method is the same as that of Example 1; the difference is that in the preparation method of the admixture, the method for preparing the counterion quaternary ammonium salt in step (2) is: directly mixing methyl carbonate quaternary ammonium salt and octanoic acid to obtain.

[0152] Performance Testing Methods

[0153] With reference to GB / T 50081-2019 “Standard for Test Methods for Physical and Mechanical Properties of Concrete”, relevant mechanical properties tests were carried out on the examples and comparative samples.

[0154] The compressive strength test method after corrosion is: soak the concrete sample after curing for 28 days in a sodium sulfate aqueous solution with a mass concentration of 5%, and test the compressive strength after soaking for 90 days.

[0155] Corrosion resistance retention rate = compressive strength 90d / Compressive Strength 28d *100%;

[0156] Refer to GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" for anti-permeability test.

[0157] The test results of the examples and comparative examples are shown in Table 1.

[0158] Performance test data

[0159] Table 1. Performance test results

[0160]

[0161]

[0162] It can be seen from the test results that the concrete obtained in Examples 1-5 has good compressive strength, corrosion resistance and permeability resistance, indicating that the influence of admixtures on the strength, permeability and corrosion resistance of concrete is crucial. The specific analysis is as follows:

[0163] In Example 4, the amount of octanoic acid added is relatively low, and various properties of the concrete are reduced. It is speculated that the organic carboxylate calcium generated in situ by the admixture and the calcium ions in the system is relatively small, resulting in a decrease in the density of the concrete system, and there may not be enough excess carboxylates in the admixture to be grafted onto the carbon fibers, resulting in poor dispersion uniformity of the carbon fibers, which also leads to a decrease in the continuity of the conductive network in the system. Therefore, the compressive strength, corrosion resistance and impermeability of the product are all reduced.

[0164] In Example 5, the addition amount of octanoic acid is relatively high, and the various properties of the concrete do not change much. This may be because when the addition amount of methyl carbonate quaternary ammonium salt is constant, adding too much octanoic acid will not increase the counter ion end content on the quaternary ammonium salt, that is, the addition amount of octanoic acid has reached the saturation level, and adding more has little effect on the overall performance.

[0165] In Comparative Example 1, no admixture was added, and the various properties of the concrete were significantly deteriorated. The reason may be that not adding admixtures is not conducive to the protection of the steel bars, and the density of the concrete system is reduced, so the compressive strength, corrosion resistance and impermeability of the product are significantly reduced.

[0166] In Comparative Example 2, only methyl carbonate quaternary ammonium salt is introduced as an admixture, and the performance is reduced compared with the counterion quaternary ammonium salt. It is speculated that since there is only methyl carbonate quaternary ammonium salt in the admixture, it does not have a part that can react with calcium ions in the system to generate organic carboxylic acid calcium, and the internal pore structure of the concrete cannot be further optimized, resulting in a decrease in the density of the concrete system. At the same time, it cannot cooperate with carbon fiber to build a conductive network, and the cathodic protection effect on the steel bar is lost, so the compressive strength, corrosion resistance and permeability resistance of the product are all reduced.

[0167] The performance of the sample obtained in Comparative Example 3 deteriorates, and the reason may be that the carboxylic acid selected for preparing the counter-ion quaternary ammonium salt is propionic acid, which gives the admixture a shorter counter-ion chain, which not only reduces its own hydrophobicity and weakens its anti-permeability performance; but also because the carbon chain is too short, its effect on the uniformity of carbon fiber dispersion deteriorates, and the degree of interweaving with the conductive network built by carbon fibers deteriorates, so the compressive strength and corrosion resistance of the product are reduced.

[0168] The performance of the sample obtained in Comparative Example 4 deteriorates, and the reason may be that the carboxylic acid selected for preparing the counter-ion quaternary ammonium salt is myristic acid, and the counter-ion chain length in the obtained admixture is longer, and its own hydrophobicity becomes better, which is beneficial to the anti-permeability of the concrete; however, the longer chain length may cause long chain winding, and even if organic calcium carboxylate is generated to fill the gap, its non-uniformity is high, which is not conducive to the improvement of the overall density of the concrete, not only affecting the strength, but also affecting the anti-permeability to a certain extent, and the curling and winding of the long chain will affect the arrangement of the carbon fibers, and the degree of interweaving of the conductive network becomes worse, so the compressive strength and corrosion resistance of the product are reduced.

[0169] The performance of the sample obtained in Comparative Example 5 deteriorates, and the reason may be that: octanoic acid and methyl carbonate quaternary ammonium salt are directly mixed, and octanoic acid is directly added, which is difficult to react with calcium ions to form organic calcium carboxylate. The carboxylic acid that is not grafted with the quaternary ammonium salt has disordered curling and entanglement of the alkyl long chain, and cannot cooperate well with the carbon fiber to construct a conductive network. Therefore, the compressive strength, corrosion resistance and impermeability resistance of the product are significantly reduced.

Claims

1. A concrete for pipe piles containing ultrafine powder, characterized in that: The raw materials for preparing the concrete for pipe piles include, by weight: 190-500 parts of cement, 550-1400 parts of coarse aggregate, 300-800 parts of fine aggregate, 40-110 parts of ultrafine powder, 20-50 parts of admixture, 12-35 parts of carbon fiber, 2-9 parts of water reducer, and 70-180 parts of water; The additive is a counter-ion quaternary ammonium salt.

2. The ultrafine powder-containing concrete for pipe piles according to claim 1, characterized in that: The additive accounts for 2-15wt% of the total amount of the gel material; preferably 3-12wt%; more preferably 5-10wt%; The gel material consists of cement and superfine powder.

3. The ultrafine powder-containing concrete for pipe piles according to claim 1, characterized in that: The raw materials for preparing the counterion quaternary ammonium salt include methyl carbonate quaternary ammonium salt and carboxylic acid; Preferably, the mass ratio of the methyl carbonate quaternary ammonium salt to the carboxylic acid is 1:(0.1-0.5); More preferably, the mass ratio of the methyl carbonate quaternary ammonium salt to the carboxylic acid is 1:(0.20-0.35).

4. The ultrafine powder-containing concrete for pipe piles according to claim 3, characterized in that: The raw materials for preparing the methyl carbonate quaternary ammonium salt include dialkyl methyl tertiary amine and dimethyl carbonate; The dialkylmethyl tertiary amine includes C5-C 20 Dialkylmethyl tertiary amine; Preferably, the dialkylmethyl tertiary amine is C 10 -C 16 Dialkylmethyl tertiary amine; More preferably, the dialkylmethyl tertiary amine is at least one of dioctylmethyl tertiary amine, didecylmethyl tertiary amine, didodecylmethyl tertiary amine, didetradecylmethyl tertiary amine, and didhexadecylmethyl tertiary amine.

5. The ultrafine powder-containing concrete for pipe piles according to claim 3, characterized in that: The chain length of the carboxylic acid is C2-C 18 Preferably, the chain length of the carboxylic acid is C3-C 12 More preferably, the chain length of the carboxylic acid is C6-C 10 .

6. The ultrafine powder-containing concrete for pipe piles according to claim 1, characterized in that: In terms of weight, the ultrafine powder includes: 15-40 parts of slag, 10-30 parts of fly ash, 10-30 parts of slaked lime, and 5-10 parts of silica fume.

7. The ultrafine powder-containing concrete for pipe piles according to claim 1, characterized in that: The carbon fiber has a length of 1-10 mm and a diameter of 5-15 μm.

8. The ultrafine powder-containing concrete for pipe piles according to claim 1, characterized in that: The water reducer includes at least one of a naphthalene-based water reducer, a sulfonate-based water reducer, a polycarboxylic acid-based water reducer, and an amino-based water reducer.

9. The ultrafine powder-containing concrete for pipe piles according to claim 1, characterized in that: The preparation method of the admixture is as follows: adding methyl carbonate quaternary ammonium salt to a solvent, stirring continuously at 20-75° C., adding carboxylic acid while stirring after the methyl carbonate quaternary ammonium salt is completely dissolved, stirring for 10-240 minutes; then recrystallizing, drying to constant weight, and obtaining an admixture product.

10. A method for preparing ultrafine powder-containing concrete for pipe piles, characterized in that: The preparation steps of the concrete for pipe piles include: 1) mixing cement, coarse aggregate, fine aggregate, ultrafine powder, carbon fiber, water reducer and water, and stirring evenly to obtain a mixture; 2) adding an admixture to the mixture prepared in step 1), stirring evenly to obtain concrete for pipe piles.

Citation Information

Patent Citations

  • A high-strength impermeable concrete and its production method

    CN108623265B