Large-volume muck high-flow-state filling material and preparation method thereof
Through large amounts of slag high-fluid filling materials, combined with nano-scale bubbles and other additives, the problems of poor fluidity and high cost of traditional filling materials are solved, and low-cost and efficient filling of karst areas and goaf areas are achieved, and the basics are improved. Governance capabilities of facilities.
Patent Information
- Application Number
- CN202410983084.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-22
AI Technical Summary
In karst areas and goaf areas, traditional filling materials have poor mobility and high cost, resulting in low efficiency in subsidence or collapse management of infrastructure, affecting the safety and extension of the transportation network.
High-flow filling materials are used for large amounts of slag, and the composition includes sulfate cement, slag, fly ash, sodium tripolyphosphate, sodium dodecane sulfate, 2-ethylhexylphosphate-2-ethylhexylphosphate, Nano-scale bubbles, polyacrylamide and calcium formate are prepared by hydrocatalysis to improve the fluidity and strength of the material, reduce viscosity, and enhance compressive and impermeability resistance.
Low-cost and high-flow filling of infrastructure undervoltage goaf has been achieved, filling efficiency and quality has been improved, and efficient material management capabilities have been ensured.
Abstract
Description
Technical Field
[0001] The invention relates to the field of underground engineering, and in particular to a high-fluidity filling material with a large amount of slag and a preparation method thereof. Background Art
[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] Karst areas account for nearly 1 / 3 of my country's land area, and the area of underground goafs is as high as 1.349 million hectares. Major transportation infrastructure such as rail transit inevitably passes through disaster sources such as karst and goafs, and is prone to large-scale subsidence or collapse, becoming a "stuck point" and "pain point" that restricts the density and extension of transportation networks. Especially for high-speed railways, slight subsidence will seriously affect operational safety. Traditional filling materials have poor fluidity and high cost, which greatly affects filling efficiency and filling quality. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a high-fluidity filling material with a large amount of slag and a preparation method thereof, which can achieve low-cost and high-fluidity filling of the goaf beneath the infrastructure, thereby achieving efficient management of the goaf beneath the infrastructure.
[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0006] In a first aspect, the present invention provides a high-fluidity filling material with a large amount of slag, which is composed of the following components, measured by mass: 8 to 10 parts of sulfate cement, 80 to 100 parts of slag, 16 to 20 parts of fly ash, 0.2 to 0.4 parts of sodium tripolyphosphate, 0.4 to 0.5 parts of sodium dodecyl sulfate, 0.3 to 0.4 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.2 to 0.3 parts of nano-bubbles, 0.1 to 0.2 parts of polyacrylamide, 0.6 to 0.9 parts of calcium formate, and 12 to 18 parts of water.
[0007] The functions of each component are:
[0008] Sulfate cement: provides strength, increases the hardness and compressive strength of the filling material, and provides better agglomeration and impermeability properties.
[0009] Muck: It is conventional engineering muck. It supports the skeleton and improves the compressive strength of the material.
[0010] As a kind of construction waste, slag is often dumped and discarded at will, causing environmental pollution. Using slag as the main aggregate of materials and recycling waste can greatly save material costs. Fly ash, sodium tripolyphosphate and sodium dodecyl sulfate can ensure high fluidity even with a large amount of fly ash.
[0011] Fly ash: One of the sources of material strength, it can also improve the fluidity, cohesion and water retention of the material, making the material easy to pump and shape.
[0012] Sodium tripolyphosphate: Promotes the absorption of water in cement, improves the fluidity and ductility of cement, thereby enhancing the strength and toughness of the material; improves the material's anti-permeability.
[0013] Sodium dodecyl sulfate: reduces the viscosity of the material, making it easier to construct and flow; increases the flexibility and plasticity of the material, thereby improving its crack resistance; promotes the early hydration reaction of the mortar, allowing it to reach a hardened state faster.
[0014] 2-Ethylhexyl Phosphate: Stimulates the activity of admixtures in the material, effectively improves the fluidity of the material, and improves the cohesiveness of the material.
[0015] Nano-scale bubbles: improve material toughness; increase material compressive strength; reduce material porosity and improve material durability.
[0016] Polyacrylamide: It has water-retaining properties, making the material less likely to disperse; it enhances the material's impermeability and bonding strength; it improves the material's tensile and bending resistance, durability and bending toughness.
[0017] Calcium formate: increases the early strength of the material, accelerates cement curing, and shortens the setting time;
[0018] In some embodiments, the high-fluidity filling material with a large amount of slag is composed of the following components, measured by mass: 8-10 parts of sulfate cement, 85-95 parts of slag, 16-20 parts of fly ash, 0.2-0.4 parts of sodium tripolyphosphate, 0.4-0.5 parts of sodium dodecyl sulfate, 0.3-0.4 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.2-0.3 parts of nano-bubbles, 0.1-0.2 parts of polyacrylamide, 0.6-0.9 parts of calcium formate, and 12-16 parts of water.
[0019] In some embodiments, the nano-sized bubbles are prepared by hydrodynamic cavitation. When the airflow and water flow pass through the neck of the venturi tube, the pressure changes rapidly due to the sharp decrease in the tube diameter, and the millimeter-sized bubbles quickly burst and collapse into micro-nano-sized bubbles.
[0020] Preferably, the diameter of the nano-sized bubbles is less than 200 nm.
[0021] In some embodiments, the molecular weight of polyacrylamide is 10 million to 18 million.
[0022] The viscosity of polyacrylamide solution increases with the increase of polymer molecular weight. A molecular weight of 10 million to 18 million can achieve the best effect required by the material and maximize the strength of the material.
[0023] In some embodiments, the specific surface area of sulphoaluminate cement is 400 to 600 m 2 / kg. The setting time of this cement with a water-cement ratio of 0.5 is 5 to 20 minutes.
[0024] In some embodiments, the particle size of the slag is 2 mm-10 mm.
[0025] Preferably, the particle size of the slag is 4mm-7mm.
[0026] In a second aspect, the present invention provides a method for preparing the high-fluidity filling material with a large amount of slag, comprising the following steps:
[0027] Grind and crush large particles;
[0028] Nano-bubble water is produced by hydrodynamic cavitation;
[0029] The product is obtained by uniformly mixing the components according to the preset mass ratio.
[0030] In some embodiments, the solid powders are first mixed evenly and then mixed with the nano-scale bubble water.
[0031] The beneficial effects achieved by one or more embodiments of the present invention are as follows:
[0032] The filling material of the present invention has good fluidity and realizes high-efficiency and low-cost filling of the goaf. DETAILED DESCRIPTION
[0033] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0034] The present invention will be further described below in conjunction with the embodiments.
[0035] Example 1
[0036] A high-fluidity filling material with a large amount of slag soil is composed of the following components in parts by mass: 10 parts of sulfate cement, 80 parts of slag soil, 20 parts of fly ash, 0.2 parts of sodium tripolyphosphate, 0.4 parts of sodium dodecyl sulfate, 0.3 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.3 parts of nano-bubbles, 0.1 parts of polyacrylamide, 0.9 parts of calcium formate, and 15 parts of water.
[0037] The selected sulphoaluminate cement setting time is 10 min, and the fly ash specific surface area is 500 m 2 / kg, density 2.4g / cm 3 The average diameter of nano-bubbles is 150nm, and the molecular weight of polyacrylamide is 15 million.
[0038] The components are mixed evenly in proportion to form a high-fluidity filling material with a large amount of slag.
[0039] According to NB / T 51070-2017 "Test methods for coal mine paste filling materials", the initial and final setting time, fluidity and uniaxial compressive strength of the filling materials were tested.
[0040] The slurry prepared according to the above ratio has an initial setting time of 6 hours, a final setting time of 12 hours, a truncated cone flow distance of 18 cm, a 3d compressive strength of 7.5 MPa, and a 28-day compressive strength of 10 MPa.
[0041] Example 2
[0042] A high-fluidity filling material with a large amount of slag soil is composed of the following components in parts by mass: 10 parts of sulfate cement, 80 parts of slag soil, 20 parts of fly ash, 0.2 parts of sodium tripolyphosphate, 0.3 parts of nano-level bubbles, 0.1 parts of polyacrylamide, 0.9 parts of calcium formate, and 15 parts of water.
[0043] The selected sulphoaluminate cement setting time is 10 min, and the fly ash specific surface area is 500 m 2 / kg, density 2.4g / cm 3 , the diameter of nano-bubbles is 150nm, and the molecular weight of polyacrylamide is 15 million.
[0044] The components are mixed evenly in proportion to form a high-fluidity filling material with a large amount of slag.
[0045] The slurry prepared according to the above ratio has an initial setting time of 6.5h, a final setting time of 13h, a truncated cone flow distance of 17cm, a 3d compressive strength of 7MPa, and a 28-day compressive strength of 9.5MPa.
[0046] Example 3
[0047] A high-fluidity filling material with a large amount of slag soil is composed of the following components in parts by mass: 10 parts of sulfate cement, 80 parts of slag soil, 20 parts of fly ash, 0.2 parts of sodium tripolyphosphate, 0.4 parts of sodium dodecyl sulfate, 0.3 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.3 parts of nano-bubbles, 0.1 parts of polyacrylamide, and 15 parts of water.
[0048] The selected sulphoaluminate cement setting time is 10 min, and the fly ash specific surface area is 500 m2 / kg, density 2.4g / cm 3 , the diameter of nano-bubbles is 150nm, and the molecular weight of polyacrylamide is 15 million.
[0049] The components are mixed evenly in proportion to form a high-fluidity filling material with a large amount of slag.
[0050] The slurry prepared according to the above ratio has an initial setting time of 6.5h, a final setting time of 12h, a truncated cone flow distance of 17.5cm, a 3d compressive strength of 7.2MPa, and a 28-day compressive strength of 9.8MPa.
[0051] Comparative Example 1
[0052] The difference from Example 1 is that 2-ethylhexyl phosphate-2-ethylhexyl ester is omitted. Other aspects are the same as Example 1.
[0053] The prepared slurry has an initial setting time of 6.5 h, a final setting time of 13 h, a truncated cone flow distance of 17 cm, a 3d compressive strength of 7.4 MPa, and a 28-day compressive strength of 9.8 MPa.
[0054] Comparative Example 2
[0055] The difference from Example 1 is that the nano-sized bubbles are omitted. The other aspects are the same as those of Example 1.
[0056] The prepared slurry has an initial setting time of 6 h, a final setting time of 12 h, a truncated cone flow distance of 18 cm, a 3d compressive strength of 7 MPa, and a 28-day compressive strength of 9 MPa.
[0057] Comparative Example 3
[0058] The difference from Example 1 is that fly ash is omitted. Other aspects are the same as Example 1.
[0059] The prepared slurry has an initial setting time of 8 h, a final setting time of 15 h, a truncated cone flow distance of 15 cm, a 3d compressive strength of 5 MPa, and a 28-day compressive strength of 7 MPa.
[0060] Comparative Example 4
[0061] The difference from Example 1 is that sodium tripolyphosphate is omitted. Other aspects are the same as those of Example 1.
[0062] The prepared slurry had an initial setting time of 6.5 h, a final setting time of 13.5 h, a truncated cone flow distance of 16.5 cm, a 3d compressive strength of 7.2 MPa, and a 28-day compressive strength of 9.5 MPa.
[0063] Comparative Example 5
[0064] The difference from Example 1 is that sodium dodecyl sulfate is omitted. Other aspects are the same as Example 1.
[0065] The prepared slurry had an initial setting time of 6.6 h, a final setting time of 13.8 h, a truncated cone flow distance of 16.4 cm, a 3d compressive strength of 7.3 MPa, and a 28-day compressive strength of 9.7 MPa.
[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-fluidity filling material with a large amount of slag, characterized by: The invention is composed of the following components in parts by mass: 8 to 10 parts of sulfate cement, 80 to 100 parts of slag, 16 to 20 parts of fly ash, 0.2 to 0.4 parts of sodium tripolyphosphate, 0.4 to 0.5 parts of sodium dodecyl sulfate, 0.3 to 0.4 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.2 to 0.3 parts of nano-bubbles, 0.1 to 0.2 parts of polyacrylamide, 0.6 to 0.9 parts of calcium formate and 12 to 18 parts of water.
2. The high-fluidity filling material with large amount of slag according to claim 1 is characterized in that: The invention is composed of the following components by mass: 8-10 parts of sulfate cement, 85-95 parts of slag, 16-20 parts of fly ash, 0.2-0.4 parts of sodium tripolyphosphate, 0.4-0.5 parts of sodium dodecyl sulfate, 0.3-0.4 parts of 2-ethylhexyl phosphate-2-ethylhexyl ester, 0.2-0.3 parts of nano-bubbles, 0.1-0.2 parts of polyacrylamide, 0.6-0.9 parts of calcium formate and 12-16 parts of water.
3. The high-fluidity filling material with large amount of slag according to claim 1 is characterized in that: The method for preparing nano-scale bubbles is: preparing them by adopting a hydrodynamic cavitation method.
4. The high-fluidity filling material with large amount of slag according to claim 1 is characterized in that: The diameter of nanobubbles is less than 200nm.
5. The high-fluidity filling material with large amount of slag according to claim 1 is characterized in that: The molecular weight of polyacrylamide is 10 million to 18 million.
6. The high-fluidity filling material with large amount of slag according to claim 1 is characterized in that: Sulphoaluminate cement specific surface area 400~600m 2 / kg. The setting time of this cement with a water-cement ratio of 0.5 is 5 to 20 minutes.
7. The high-fluidity filling material with large amount of slag according to claim 1 is characterized by: The particle size of the slag is 2mm-10mm.
8. The high-fluidity filling material with large amount of slag according to claim 1 is characterized by: The particle size of the slag is 4mm-7mm.
9. The method for preparing the high-fluidity filling material with a large amount of slag as claimed in any one of claims 1 to 8, characterized in that: The steps include: Grind and crush large particles; Nano-bubble water is produced by hydrodynamic cavitation; The product is obtained by uniformly mixing the components according to the preset mass ratio.
10. The method for preparing a high-fluidity filling material with a large amount of slag according to claim 9, characterized in that: Firstly, mix all the solid powders evenly, and then mix them with the nano-level bubble water.
Citation Information
Patent Citations
Original-state shield muck flow-state filler as well as preparation method and application thereof
CN117361959A
Novel green dispersion-resistant synchronous grouting material for water-rich stratum and preparation method of novel green dispersion-resistant synchronous grouting material
CN117865593A