Method for preparing gypsum-based self-leveling mortar from coal gangue and chemical gypsum

By combining modified coal gangue and chemical gypsum, high-thermal conductivity and high-strength gypsum-based self-leveling mortar was prepared, which solved the problem of insufficient thermal conductivity of gypsum-based self-leveling mortar in the prior art, and achieved efficient search for floor heating Peaceful insulation effect.

CN118908682APending Publication Date: 2024-11-08SHAANXI YUNENG QINGQINGYUAN ENVIRONMENTAL PROTECTION MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410590425.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing gypsum-based self-leveling mortar is insufficient in floor heating applications, which leads to hollowing and cracking of the mortar, which cannot meet the requirements of alternating changes in the cold and heat.

Method used

Modified coal gangue and chemical gypsum are used to prepare high-thermal conductivity and high-strength gypsum-based self-leveling mortar with porous modification, decolorization and low-temperature calcination, combined with exciter, water reducing agent, suspension agent, defoaming agent and retarder. , reduce the firing temperature and improve the looseness of the material.

Benefits of technology

It has achieved low energy consumption to prepare lightweight, high thermal conductivity and high strength self-leveling sand material, suitable for floor heating and non-floor heating leveling. The material has a large thermal conductivity, small volume density, and small dimensional change rate. It is suitable for use as a cushion layer, insulation layer and surface layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004837100120000071
    Figure BDA0004837100120000071
  • Figure BDA0004837100120000081
    Figure BDA0004837100120000081
Patent Text Reader

Abstract

The invention discloses a method for preparing gypsum-based self-leveling mortar from coal gangue and chemical gypsum, and relates to the technical field of building materials. The concrete is prepared from the following components: chemical gypsum, modified coal gangue, a water reducing agent, a suspending agent, a defoaming agent, an exciting agent and a retarder, the preparation method comprises the following steps: S1, carrying out porous modification and decoloration on coal gangue by using a modifier to modify the coal gangue; s2, mixing the modified coal gangue and chemical gypsum, and blending with an exciting agent to prepare pretreated powder; s3, calcining the pretreated powder at the temperature of 300-500 DEG C to obtain main powder after calcining is completed; s4, mixing the main powder with a water reducing agent, a suspending agent, a defoaming agent and a retarder to obtain the self-leveling sand material; the exciting agent and the modifying agent act together to reduce the firing temperature of the pretreated powder; the purpose of preparing the lightweight high-thermal-conductivity high-strength self-leveling sand material with low energy consumption is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a method for preparing gypsum-based self-leveling mortar by using coal gangue and chemical gypsum. Background Art

[0002] At present, the fillers commonly used in self-leveling gypsum are quartz sand, quartz powder, calcium carbonate machine-made sand, and calcium carbonate powder. The thermal conductivity of quartz sand and quartz powder is about 1.3W / m·k, which is generally used for self-leveling gypsum on floor heating. It conducts heat quickly and evenly, and the leveling layer is not prone to cracking, but it is expensive; calcium carbonate machine-made sand and calcium carbonate powder are cheaper than quartz sand and quartz powder, but the thermal conductivity is low, about 0.05W / m·k, and is generally used for the cushion or surface leveling of non-floor heating self-leveling gypsum.

[0003] China's public patent CN107935487 A records a self-leveling mortar, the formula of which includes 10% clinker, 20% coal gangue, 20% red mud, 40% stone powder, 10% gypsum, and 1.5% activator. However, in the prior art, it is only prepared by physical mixing, and its strength after curing is low. At the same time, there is no targeted improvement in the thermal conductivity of the finished product after curing to cope with the increasingly common situation of floor heating.

[0004] Gypsum-based self-leveling mortar was initially used only for self-leveling of the ground, and the emphasis has always been on fluidity and strength, as well as hollowing and cracking for cement-based self-leveling, that is, the parameter control of the size change rate. However, with the expansion of market applications and the popularization of buried floor heating in the leveled ground, the general characteristics of gypsum-based self-leveling mortar cannot meet the new requirements given by the market. The gypsum-based self-leveling mortar used for floor heating must have a higher thermal conductivity than ordinary gypsum-based self-leveling mortar in the alternating changes of extreme cold and extreme heat, otherwise it is very easy to cause hollowing and cracking of the mortar.

[0005] Coal gangue is a kind of black-gray solid waste discharged during coal mining or coal washing, which is harder than coal and has a low carbon content. It is a mixture of carbonaceous, argillaceous and sandy shale, with a carbon content of 20% to 30%, a low calorific value of 2090 to 4180 KJ / kg, a hardness equivalent to limestone, about 3, and a lower density than limestone, at 1.6 g / cm 3 . Summary of the invention

[0006] The object of the present invention is to provide a method for preparing gypsum-based self-leveling mortar by using coal gangue and chemical gypsum, so as to achieve the purpose of preparing a light, high-thermal-conductivity and high-strength self-leveling sand material with low energy consumption.

[0007] In order to achieve the above object, the present invention adopts the following technical means:

[0008] A method for preparing gypsum-based self-leveling mortar using coal gangue and chemical gypsum, comprising the following components: chemical gypsum, modified coal gangue, water reducing agent, suspending agent, defoaming agent, activator and retarder;

[0009] Prepared in the following way:

[0010] S1. Using a modifier to modify the coal gangue to be porous and decolorized, so as to modify the coal gangue;

[0011] S2. The modified gangue and chemical gypsum are mixed and blended with an activator to obtain a pretreated powder;

[0012] S3. The pretreated powder is calcined at 300 to 500°C to obtain a main powder after calcination;

[0013] S4. Mix the main powder with a water reducing agent, a suspending agent, a defoaming agent and a retarder to obtain a self-leveling sand material;

[0014] The activator and the modifier work together to reduce the sintering temperature of the pretreated powder.

[0015] Preferably, the modifier is a mixed solution of a soluble decomposing salt A and a decolorizing agent B in a mass ratio of 1:1;

[0016] The soluble decomposition salt A is one of carbonate, bicarbonate and ammonium salt;

[0017] The decolorizing agent B is one of hydrogen peroxide, persulfate soluble salt, percarbonate soluble salt, and perborate soluble salt.

[0018] Furthermore, the water reducing agent is one or two of lignin sulfonate series, naphthalene series, melamine series, aminosulfonate series, aliphatic series, and polycarboxylic acid series.

[0019] Furthermore, the suspending agent is one of xanthan gum, gum arabic, carrageenan, cellulose HPMC, HEC, PVC, PVA, and PEO.

[0020] Furthermore, the defoaming agent is one of mineral oils, polyethers and silicones.

[0021] Furthermore, the activator is composed of a mixture of alkaline salts of carbonate and amine salts.

[0022] Furthermore, the retarder is one of phosphate, tartaric acid and gluconate.

[0023] Furthermore, in parts by weight, the pretreated powder is 1000 parts, the water reducer is 2-4 parts, the suspending agent is 0.4-1 parts, the defoaming agent is 0.8-1.5 parts, the activator is 8-15 parts, and the retarder is 0.5-1.5 parts.

[0024] During use, the present invention has the following beneficial effects:

[0025] Low-temperature calcination can fully utilize the calorific value of the material, saving energy while making the material looser. Through solution immersion and calcination with chemical gypsum, a gypsum-based self-leveling mortar with high thermal conductivity and light weight is prepared. The material of this technology can be used for leveling for both floor heating and non-floor heating leveling, and is widely used.

[0026] The gypsum-based self-leveling mortar prepared by the present invention has a porous structure, high thermal conductivity, low bulk density, high strength, and small dimensional change rate. It can be used not only as a cushion layer self-leveling mortar and an insulation layer self-leveling mortar, but also as a surface layer self-leveling mortar.

[0027] The activator and the modifier work together to reduce the sintering temperature of the pretreated powder.

[0028] Among them, the carbonate and alkaline salts of the activator react with the acidic components SiO2 and Al2O3 in the coal gangue to generate fluxing substances. The addition of CaSO4, the main component of gypsum, can reduce the sintering temperature of coal gangue and change its melting temperature. For example, SiO2 reacts with CaO to obtain calcium feldspar, Al2O3 reacts with CaO to generate calcium aluminate, and SiO2 and Al2O3 react with CaO to obtain calcium feldspar when they exist at the same time, which reduces the melting temperature of coal ash. The fluxing effect of these products is equivalent to that of CaO. Finally, a low-temperature eutectic is formed together with the reactants of the activator, thereby significantly reducing the melting temperature of coal gangue. Not only the hardness of coal gangue is increased, but also the volume of the sintered material is lighter due to the addition of air-entraining groups in the activator. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0030] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0032] Example 1

[0033] The abandoned coal gangue is first crushed to 8mm by a jaw crusher, and then crushed to 1mm by a hammer crusher. The coal gangue is crushed to less than 3mm, and the bulk density of the coal gangue powder is 1450Kg / cm 3 ;

[0034] The crushed gangue reacts with a modifier in a soaking tank. Specifically, the modifier is 20% soluble decomposition salt sodium carbonate and decolorizing agent sodium persulfate, which are soaked for 12 hours, and then dried and dehydrated by a dehydrator to a moisture content of less than 10% to obtain modified gangue.

[0035] The dried modified coal gangue and chemical gypsum are mixed in a weight ratio of 4:6 by an automatic weighing scale, and then blended with an activator to obtain a pretreated powder;

[0036] The pretreated powder is fed into the rotary kiln and calcined to a material temperature of 300°C. The timing is started and the material temperature is maintained at no less than 300°C for 3 hours.

[0037] The discharged material is ground by a pin mill, and the mill speed is adjusted to ensure that the particle size is not less than 0.6 mm. It is cooled to 50°C to obtain the processed main powder.

[0038] Mix 1000 parts of the main powder with 4 parts of a water reducer, 0.4 parts of a suspending agent, 0.8 parts of a defoaming agent, and 1.5 parts of a retarder to obtain a finished sand material.

[0039] The above mixing is performed using a plowshare mixer. First, half of the main powder is added to the plowshare mixer, and then other additives are added in sequence. Finally, the remaining half of the main material is added to the mixer. Mix for another 5 minutes, and then pack and store to obtain the finished sand material.

[0040] Example 2

[0041] The abandoned coal gangue is first crushed to 10mm by a jaw crusher, and then crushed to 2mm by a hammer crusher. The coal gangue is crushed to less than 3mm, and the bulk density of the coal gangue powder is 1550Kg / cm 3 ;

[0042] The crushed gangue reacts with a modifier in a soaking tank, wherein the modifier is composed of 30% soluble decomposition ammonium chloride and decolorizing agents sodium perborate and sodium percarbonate solution, soaks for 14 hours, and is dried and dehydrated by a rotary drum vacuum filter to a moisture content of less than 10% to obtain modified gangue;

[0043] The crushed modified coal gangue and chemical gypsum are mixed in a weight ratio of 5:5 by an automatic weighing scale, and blended with an activator to obtain a pretreated powder;

[0044] The pretreated powder is fed into a rotary kiln and calcined to a material temperature of 400°C. The timing is started and the material temperature is maintained at no less than 400°C for 2.5 hours.

[0045] The discharged material is ground through a claw type crusher (do not put a screen on the inner wall), and the mill speed is adjusted to ensure that the particle size is not less than 0.6mm. It is cooled to 50℃ to obtain the processed main powder.

[0046] 1000 parts of main powder, 3 parts of water reducing agent, 0.6 parts of suspending agent, 1.2 parts of defoaming agent and 1.2 parts of retarder are mixed to obtain finished sand material.

[0047] The above mixing is carried out by a plowshare mixer, first adding half of the main material into the plowshare mixer, then adding the formula additives in sequence, and finally adding the remaining half of the main material into the mixer. Mixing for another 5 minutes, packaging and storage to obtain the finished sand material.

[0048] Example 3

[0049] The abandoned coal gangue is first crushed to 12mm by a jaw crusher, and then crushed to 3mm by a hammer crusher. The effect of crushing the coal gangue to 3mm is achieved. At this time, the bulk density of the coal gangue powder is 1600Kg / cm 3 ;

[0050] The crushed gangue is soaked in a soaking tank with a modifier for reaction. In this embodiment, the modifier is composed of 40% soluble decomposition salt sodium bicarbonate and decolorizing agent hydrogen peroxide. The mixture is soaked for 18 hours and then dried and dehydrated to a moisture content of less than 10% by a horizontal screw centrifuge to obtain modified gangue.

[0051] The dried modified coal gangue and chemical gypsum are mixed in a weight ratio of 6:4 by an automatic weighing scale, and then blended with an activator to obtain a pretreated powder;

[0052] The pretreated powder is fed into a rotary kiln and calcined to a material temperature of 450°C. The timing is started and the material temperature is maintained at no less than 450°C for 2 hours.

[0053] The discharged material is ground through a ball mill (do not start the powder selector), the mill speed is adjusted to ensure that the particle size is not less than 0.6mm, and cooled to 50℃ to obtain the processed main powder.

[0054] Mix the main powder and formulation additives in the following parts by weight: 1000 parts of main powder, 2 parts of water reducing agent, 0.8 parts of suspending agent, 1.4 parts of defoaming agent, and 1 part of retarder.

[0055] Mixing is performed in the following manner: start the plowshare mixer, first add half of the main material into the plowshare mixer, then add the formulation additives in sequence, and finally add the remaining half of the main material into the mixer. Mix for another 5 minutes, and then package and store to obtain the finished sand material.

[0056] Comparative Example 1

[0057] In this comparative example, the coal gangue is not soaked with the modifier, and no activator is added, and the rest is the same as Example 1.

[0058] Comparative Example 2

[0059] In this comparative example, the coal gangue is not soaked with the modifier, and no activator is added, and the rest is the same as Example 2.

[0060] Comparative Example 3

[0061] In this comparative example, the coal gangue is not soaked with the modifier, and no activator is added, and the rest is the same as Example 3.

[0062] Comparative Example 4

[0063] In this comparative example, the main powders are limestone and gypsum, and the rest are the same as those in Example 1.

[0064] Comparative Example 5

[0065] In this comparative example, the main powders are limestone and gypsum, and the rest are the same as those in Example 2.

[0066] Comparative Example 6

[0067] In this comparative example, the main powders are limestone and gypsum, and the rest are the same as those in Example 3.

[0068] According to the method of JC / T 1023-2021 "Gypsum-based self-leveling mortar", the above embodiments and comparative examples were tested respectively, and the performance index values ​​are as follows:

[0069]

[0070]

[0071] From the above table, it can be found that when no modifier and activator are added, the main powder cannot achieve good sintering because the sintering temperature is difficult to reach the sintering temperature of the main powder. During the sintering process, a small amount of micropores can still be generated, and the micropores generated in this way will have a greater impact on the strength and thermal conductivity of the material. During low-temperature sintering, it cannot be completely sintered, resulting in the thermal conductivity and strength of the finished material being lower than the material of the present invention. In addition, due to the small number of micropores formed, its volume density is large, so it is difficult to achieve the purpose of light weight.

[0072] At the same time, for the comparative example using limestone and gypsum as the main powder, even if an activator and a modifier are added, the volume density is still higher than the material involved in the present invention, but slightly lower than the materials prepared in comparative examples 1 to 3. However, it has a greater impact on thermal conductivity and is difficult to adapt to an environment requiring a high thermal conductivity coefficient.

[0073] Moreover, the strength of the above-mentioned embodiment is obviously much higher than that of the comparative example, and the embodiment is light in weight, small in volume density, very small in dimensional change rate, and large in thermal conductivity, which is suitable for self-leveling mortar. Due to its large thermal conductivity, it heats up faster, has less heat accumulation, and is not easy to crack, so it is also very suitable for self-leveling of pouring floor heating.

[0074] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing gypsum-based self-leveling mortar using coal gangue and chemical gypsum, characterized in that: It is composed of the following ingredients: chemical gypsum, modified coal gangue, water reducing agent, suspending agent, defoaming agent, activator and retarder; Prepared in the following manner: S1. Using a modifier to modify the coal gangue to be porous and decolorized, so as to modify the coal gangue; S2. The modified gangue and chemical gypsum are mixed and blended with an activator to obtain a pretreated powder; S3. The pretreated powder is calcined at 300 to 500°C to obtain a main powder after calcination; S4. The main powder is mixed with a water reducing agent, a suspending agent, a defoaming agent and a retarder to obtain a self-leveling sand material; the activator and the modifier work together to reduce the sintering temperature of the pretreated powder.

2. The method for preparing gypsum-based self-leveling mortar using coal gangue and chemical gypsum according to claim 1, characterized in that: The modifier is a mixed solution of a soluble decomposing salt A and a decolorizing agent B in a mass ratio of 1:1; The soluble decomposition salt A is one of carbonate, bicarbonate and ammonium salt; The decolorizing agent B is one of hydrogen peroxide, persulfate soluble salt, percarbonate soluble salt, and perborate soluble salt.

3. The method for preparing gypsum-based self-leveling mortar using coal gangue and chemical gypsum according to claim 1, characterized in that: The water reducing agent is one or two of lignin sulfonate series, naphthalene series, melamine series, aminosulfonate series, aliphatic series, and polycarboxylic acid series.

4. The method for preparing gypsum-based self-leveling mortar using coal gangue and chemical gypsum according to claim 1, characterized in that: The suspending agent is one of xanthan gum, gum arabic, carrageenan, cellulose HPMC, HEC, PVC, PVA, and PEO.

5. The method for preparing gypsum-based self-leveling mortar using coal gangue and chemical gypsum according to claim 1, characterized in that: The defoaming agent is one of mineral oil, polyether and silicone.

6. The method for preparing gypsum-based self-leveling mortar using coal gangue and chemical gypsum according to claim 1, characterized in that: The activator is composed of a mixture of alkaline salts of carbonate and amine salts.

7. The method for preparing gypsum-based self-leveling mortar using coal gangue and chemical gypsum according to claim 1, characterized in that: The retarder is one of phosphate, tartaric acid and gluconate.

8. The method for preparing gypsum-based self-leveling mortar using coal gangue and chemical gypsum according to any one of claims 1 to 7, characterized in that: In parts by weight, the pretreatment powder is 1000 parts, the water reducer is 2-4 parts, the suspending agent is 0.4-1 parts, the defoamer is 0.8-1.5 parts, the activator is 8-15 parts, and the retarder is 0.5-1.5 parts.