Preparation method of mullite thermal insulation material with infrared reflecting layer
Through the layer-by-layer assembly process, the centralized distribution and layered arrangement of potassium hexatitate whiskers are formed in the fiber thermal insulation material, which solves the complex problems of infrared reflective layer design and process in the prior art, and improves the thermal insulation performance of the material and high temperature stability simplify the process flow.
Patent Information
- Application Number
- CN202410958462.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The method of introducing potassium hexatitate whiskers into existing fiber insulation materials has problems such as homogenous materials that are not conducive to centralized distribution of whiskers, poor material designability and complex process, especially the design and process of infrared reflective layers are difficult to achieve in the material. Effective internal integration.
Using layer-by-layer assembly process, mullite fibers and potassium hexattitanate whiskers are dispersed into deionized water and binder. Through the slurry, a three-layer structure of upper, middle and lower are formed, using hexattitanate. The density characteristics of potassium whiskers allow it to settle to the intermediate layer, forming an infrared reflective layer, and improving the high temperature stability and thermal insulation ability of the material through the layered arrangement of fibers and whiskers.
The centralized distribution and layered arrangement of potassium hexititate whiskers are achieved, which improves the infrared reflection performance and high temperature stability of the material, reduces the high temperature thermal conductivity, avoids the loss caused by the direct contact of the whiskers with heat sources, and simplifies the The process flow enhances the design of the material.
Smart Images

Figure CN118908689A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a mullite heat insulating material. Background Art
[0002] In recent years, for the purpose of energy conservation and the needs of the aerospace industry, people have put forward higher requirements on the performance of thermal insulation materials. Porous fibrous thermal insulation materials are composed of randomly overlapped fibers and binders on the fiber nodes to form a stable three-dimensional network structure. They have excellent properties such as low density, high elasticity, high porosity, low thermal conductivity, good high temperature stability, low elastic modulus and good resistance to thermal shock, and have become one of the important candidate materials for thermal insulation needs in the aerospace field.
[0003] The thermal insulation capacity of mullite fiber insulation materials at high temperatures is not very ideal, and adding infrared reflectors is an effective solution. Potassium hexatitanate whiskers are an excellent infrared reflector. It has a high melting point, which can reach 1350℃~1370℃; its tunnel-like structure gives it structural thermal insulation performance; and its infrared reflectivity is high, which is greater than 70% in the wavelength range of 400nm~2600nm and close to 100% in the wavelength range of 700nm~750nm. Introducing potassium hexatitanate whiskers as infrared reflectors into mullite fiber insulation materials can improve their infrared reflection performance, reflect most of the heat in the infrared band, reduce the transfer of heat along the target direction, and thus reduce the high-temperature thermal conductivity of the material.
[0004] There are two existing ways to introduce potassium hexatitanate whiskers into fiber insulation material systems, and both methods have certain limitations. One is a homogeneous composite material formed by direct doping, in which the first method is to directly add potassium hexatitanate whiskers to the fiber to form a homogeneous mixed slurry, and press it to form a fibrous insulation sample; the second method is to introduce potassium hexatitanate whiskers into the matrix in a fiber reinforced resin-based or ceramic-based composite material system. Homogeneous materials are not conducive to the concentrated distribution of potassium hexatitanate whiskers and their excellent infrared reflection performance; and the material has poor designability, and the material properties can only be regulated by adjusting the whisker content. The other is to brush a coating containing potassium hexatitanate whiskers on the surface of the material. Although this method has the concept of material stratification and realizes the concentrated distribution of whiskers, it requires additional preparation of coating slurry, which increases the complexity of the process, and the application of this method is currently mostly limited to the surface of the material, and no reflective layer is added to the inside of the material. Summary of the invention
[0005] The present invention aims to solve the technical problems that in the current method of introducing potassium hexatitanate whiskers into a fiber thermal insulation material system, homogeneous materials are not conducive to the concentrated distribution of potassium hexatitanate whiskers, the material designability is poor, and additional preparation of coating slurry is required, and the process is complicated, and a method for preparing a mullite thermal insulation material with an infrared reflection layer is provided.
[0006] The preparation method of the mullite heat-insulating material with an infrared reflection layer of the present invention is carried out according to the following steps:
[0007] 1. Short-cutting of mullite fiber: The dispersibility of mullite fiber depends on the length of short-cut fiber. If the fiber length is too short, it is difficult for the fibers to overlap each other to form a three-dimensional network structure, and it is easy to form a densely packed structure, which makes the material density too high and leads to a decrease in thermal insulation performance; if the fiber length is too long, the fibers are easy to entangle and agglomerate with each other in the dispersion medium, destroying the uniformity of the slurry; therefore, it is necessary to select short-cut fibers of appropriate length;
[0008] The mullite fiber is added into deionized water, and then put into a fiber beater for short-cutting. The short-cutting time is 20min-25min. After the short-cutting is completed, it is left to stand for 20s-25s. The slag balls will sink to the bottom of the beater due to its large density and poor suspension, and it is difficult to discharge, while the fiber dispersion liquid is discharged normally, that is, the short-cutting process also removes the slag balls in the mullite fiber; the fiber is retained from the liquid outlet at the bottom of the beater, and then filtered with gauze, leaving only the fiber part, and then dried to obtain the mullite short-cut fiber;
[0009] The bottom of the inner cavity of the fiber beater is horizontal;
[0010] The mass ratio of the mullite fiber to the deionized water is 1:(100-110);
[0011] 2. Preparation of slurry:
[0012] ①, prepare the lower slurry: disperse the dried mullite chopped fibers in step 1 into the mixed solution of deionized water and binder, and stir with a stirrer for 30min to 35min to fully mix and evenly form the lower slurry;
[0013] The mass of the mullite chopped fibers is 1.5% to 2% of the mass of deionized water;
[0014] The mass of the binder is 5% to 5.5% of the mass of deionized water;
[0015] The preparation method of the upper slurry is exactly the same as that of the lower slurry;
[0016] ②, prepare infrared reflective intermediate layer slurry: disperse the dried mullite chopped fibers and potassium hexatitanate whiskers in a mixture of deionized water and a binder, and stir them with a stirrer for 30 to 35 minutes to fully mix them to form an infrared reflective intermediate layer slurry;
[0017] The mass of the potassium hexatitanate whiskers is 9% to 36% of the mass of the mullite chopped fibers;
[0018] The mass of the mullite chopped fibers is 1.5% to 2% of the mass of deionized water;
[0019] The mass of the binder is 5% to 5.5% of the mass of deionized water;
[0020] 3. ①. First, prepare the lower green sheet: pour the lower slurry prepared in step 2 into the mold, let it stand for 10-15 minutes, put a pressing sheet wrapped with gauze on the upper part of the mold, apply pressure vertically downward to the pressing sheet until the pressing sheet moves downward to the target depth, and then continue to maintain the pressure for 30-35 seconds. The excess water in the slurry flows to the top of the pressing sheet through the through hole on the pressing sheet, and then the water on the pressing sheet is taken out, and then the pressing sheet is taken out to obtain the lower green sheet in the mold;
[0021] The surface of the tablet is evenly provided with a plurality of through holes, and the diameter of the through holes is 2.5 mm to 3 mm;
[0022] The density of the green body is controlled by controlling the pressing depth of the tablet;
[0023] ②Preparation of intermediate layer green body:
[0024] 1. Slowly pour the intermediate layer slurry prepared in step 2 onto the top of the lower green sheet in the above-mentioned mold. Be careful not to disperse the lower green sheet in the mold by slowly pouring it. Let it stand for 5 to 6 minutes until the whiskers settle to the bottom. Put a pressing sheet wrapped with gauze on the top of the mold, apply pressure vertically downward to the pressing sheet until the pressing sheet moves downward to the target depth, and then continue to maintain the pressure for 30 to 35 seconds. Excess water in the slurry flows to the top of the pressing sheet through the through hole on the pressing sheet, and then the water on the pressing sheet is taken out, and then the pressing sheet is taken out to obtain the intermediate layer green sheet in the mold. The bottom of the intermediate layer green sheet is the infrared reflection layer where potassium hexatitanate whiskers are concentratedly distributed. A small amount of whiskers will adhere to the mullite fiber mesh structure during the sedimentation process.
[0025] 2. Repeat step 1 as needed to obtain multiple intermediate layers;
[0026] ③, prepare the upper green body by the same operation as step ①;
[0027] 4. Freezing and drying of slurry:
[0028] Place the mold in step 3 into a refrigerator and freeze it at -20℃ to -22℃ for 24h to 25h to ensure that the slurry is completely frozen. Then place the mold in a freeze dryer and freeze-dry for 72h to 74h to ensure that all ice crystals in the green body are sublimated to obtain a mullite thermal insulation material with an infrared reflection layer.
[0029] The present invention introduces potassium hexatitanate whiskers into a mullite fiber dispersion to form a mixed slurry, uses a layer-by-layer assembly process, and utilizes the characteristics that the density of potassium hexatitanate whiskers is greater than that of the fiber dispersion, so that most of the whiskers are settled to the bottom of the middle layer, thereby forming an infrared reflection layer where the whiskers are concentrated, and the fibers and whiskers are arranged in layers during the sedimentation process. The present invention changes the position and number of layers of the reflection layer by successive addition and molding of the slurry, thereby realizing a layered design along the thickness direction of the thermal insulation material. The material is designed to have three layers, upper, middle and lower. In actual service, the lower layer of the material is used as the hot surface. The component containing whiskers is designed in the middle layer, and the infrared reflection layer is close to the hot surface by the sedimentation of the whiskers themselves. The design of the middle layer allows the whiskers to be located inside the material instead of directly contacting the heat source. The mullite fiber provides protection for the potassium hexatitanate whiskers, reduces its service temperature, avoids the loss of the reflection layer due to long-term direct contact with the heat source, and improves the high-temperature stability of the material; the design close to the hot surface allows the heat to be reflected by the whiskers more promptly when it is transferred along the thickness direction, thereby improving the thermal insulation capacity of the material.
[0030] Advantages of introducing potassium hexatitanate whiskers into the middle of mullite fiber insulation material:
[0031] 1. Mullite fiber insulation material is deposited layer by layer with different materials along the thickness direction, that is, along the heat transfer direction. The hot surface is pure mullite fiber insulation material (i.e., the lower layer), which can meet the high temperature resistance requirements of the hot surface; the middle layer containing potassium hexatitanate whiskers is located along the heat flow, which plays a role in reflecting infrared heat energy and improving the ability of mullite fiber insulation material to resist high temperature radiation; the upper layer, i.e., the cold surface, is also mullite fiber insulation material. This low-temperature layer (cold surface) can also further reduce heat transfer in the low-temperature zone by introducing materials with lower thermal conductivity, such as silica aerogel;
[0032] 2. The potassium hexatitanate whiskers are located in the middle layer, which can prevent the potassium hexatitanate whisker powder from leaking from the mullite fiber insulation material, and avoid the disadvantage of poor physical sensation caused by the falling of powder to the user; at the same time, this method of placing the potassium hexatitanate whiskers in the middle also reduces the temperature range of the potassium hexatitanate whiskers to the medium temperature zone, which can avoid the high-temperature sintering problem of the potassium hexatitanate whiskers caused by high-temperature heat flow;
[0033] 3. The infrared reflection layer of potassium hexatitanate whiskers can be provided with multiple layers, which can further achieve the barrier to high-temperature thermal energy and improve the thermal insulation capacity of mullite fiber thermal insulation materials. The present invention can meet the demand for thermal insulation materials in different application scenarios by changing the introduction position and amount of potassium hexatitanate whiskers along the direction of heat flow transfer, thus reflecting the idea of thermal insulation structure design.
[0034] The existing method of adding potassium hexatitanate whiskers as infrared reflectors to fiber insulation materials cannot achieve concentrated distribution of whiskers, or the process is relatively complicated and limited to the surface of the material. The present invention can achieve concentrated distribution of whiskers through a simple layer-by-layer assembly process, and also performs a layered design on the inside of the material. During the sedimentation process of mullite fibers, the fiber orientation tends to be distributed along the horizontal plane, forming a three-dimensional network structure with layered distribution. Taking advantage of the fact that the density of potassium hexatitanate whiskers is greater than that of the fiber dispersion, a layered assembly process is used to make most of the potassium hexatitanate whiskers settle to the bottom and stack in layers, thereby forming an infrared reflection layer with concentrated distribution of whiskers. The present invention can change the position and number of layers of the reflection layer by the successive addition and molding of the slurry, thereby increasing the design space of the material. The reflection layer is designed in the middle layer close to the hot surface, which can be reflected by the whiskers more promptly, and avoids the loss of whiskers due to long-term direct contact with the heat source. This method does not require additional preparation of coatings, increases the protection of the whiskers, and has strong designability. In addition, at the macro level, a layered design with upper, middle, lower and infrared reflective layers was realized by using a layer-by-layer assembly process; at the micro level, the layered arrangement of fibers and whiskers was realized by using sedimentation characteristics. The macro and micro layered designs regulate the material structure at different scales.
[0035] The invention designs and optimizes the distribution of the potassium hexatitanate whisker infrared reflection layer from both macroscopic and microscopic scales with a simple process and low cost, thereby reducing the high-temperature thermal conductivity of the mullite porous fibrous material. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 A top view of the actual object of the mullite thermal insulation material with an infrared reflection layer prepared for Test 1;
[0037] Figure 2 This is a front view photo of the mullite thermal insulation material with an infrared reflection layer prepared for Experiment 1;
[0038] Figure 3 Schematic diagram of the infrared reflective intermediate layer slurry prepared in step 2 of the present invention;
[0039] Figure 4 This is a schematic diagram of the tablet after pressing down when preparing the intermediate layer green body in step 3;
[0040] Figure 5 This is a schematic diagram of the case where multiple reflective layers are required when preparing the intermediate layer green body in step 3;
[0041] Figure 6 This is a SEM image of the potassium hexatitanate whisker used in step 2 of experiment 1;
[0042] Figure 7 This is a SEM image of the upper layer of the mullite thermal insulation material with an infrared reflection layer prepared in Experiment 1;
[0043] Figure 8 This is a SEM image of the middle layer of the mullite thermal insulation material with an infrared reflection layer prepared in Experiment 1;
[0044] Fig. 9 is a graph showing the relationship between the content of potassium hexatitanate whiskers and thermal conductivity in the mullite thermal insulation material with an infrared reflection layer prepared in Experiments 1 to 5;
[0045] Fig.10 This is a graph showing the relationship between the number of infrared reflection layers and thermal conductivity in the mullite thermal insulation material with infrared reflection layers prepared in Experiments 4 and 6. DETAILED DESCRIPTION
[0046] Specific implementation method 1: This implementation method is a method for preparing a mullite thermal insulation material with an infrared reflection layer, which is specifically carried out in the following steps:
[0047] 1. Add the mullite fiber into deionized water, and then put it into the fiber beater for short-cutting. The short-cutting time is 20min-25min. After the short-cutting is completed, let it stand for 20s-25s. The fiber is retained from the liquid outlet at the bottom of the beater, and then filtered with gauze to leave only the fiber part, and then dried to obtain mullite short-cut fiber;
[0048] The bottom of the inner cavity of the fiber beater is horizontal;
[0049] The mass ratio of the mullite fiber to the deionized water is 1:(100-110);
[0050] 2. Preparation of slurry:
[0051] ①, prepare the lower slurry: disperse the dried mullite chopped fibers in step 1 into the mixed solution of deionized water and binder, and stir with a stirrer for 30min to 35min to fully mix and evenly form the lower slurry;
[0052] The mass of the mullite chopped fibers is 1.5% to 2% of the mass of deionized water;
[0053] The mass of the binder is 5% to 5.5% of the mass of deionized water;
[0054] The preparation method of the upper slurry is exactly the same as that of the lower slurry;
[0055] ②, prepare infrared reflective intermediate layer slurry: disperse the dried mullite chopped fibers and potassium hexatitanate whiskers in a mixture of deionized water and a binder, and stir them with a stirrer for 30 to 35 minutes to fully mix them to form an infrared reflective intermediate layer slurry;
[0056] The mass of the potassium hexatitanate whiskers is 9% to 36% of the mass of the mullite chopped fibers;
[0057] The mass of the mullite chopped fibers is 1.5% to 2% of the mass of deionized water;
[0058] The mass of the binder is 5% to 5.5% of the mass of deionized water;
[0059] 3. ①. First, prepare the lower green sheet: pour the lower slurry prepared in step 2 into the mold, let it stand for 10 to 15 minutes, put a pressing sheet wrapped with fine gauze on the upper part of the mold horizontally, apply pressure to the pressing sheet vertically downward until the pressing sheet moves downward to the target depth, and then continue to maintain the pressure for 30 to 35 seconds. The excess water in the slurry flows to the top of the pressing sheet through the through hole on the pressing sheet, and then the water on the pressing sheet is taken out, and then the pressing sheet is taken out to obtain the lower green sheet in the mold;
[0060] The surface of the tablet is evenly provided with a plurality of through holes, and the diameter of the through holes is 2.5 mm to 3 mm;
[0061] The density of the green body is controlled by controlling the pressing depth of the tablet;
[0062] ②Preparation of intermediate layer green body:
[0063] 1. Slowly pour the intermediate layer slurry prepared in step 2 onto the top of the lower green sheet in the above-mentioned mold, let it stand for 5 to 6 minutes until the whiskers settle to the bottom, put a pressing sheet wrapped in fine gauze on the top of the mold, apply pressure vertically downward to the pressing sheet until the pressing sheet moves downward to the target depth, and then continue to maintain the pressure for 30 to 35 seconds, and the excess water in the slurry flows to the top of the pressing sheet through the through hole on the pressing sheet, and then the water on the pressing sheet is taken out, and then the pressing sheet is taken out to obtain the intermediate layer green sheet in the mold, and the bottom of the intermediate layer green sheet is the infrared reflection layer where the potassium hexatitanate whiskers are concentratedly distributed, and a small amount of whiskers will adhere to the mullite fiber mesh structure during the sedimentation process;
[0064] 2. Repeat step 1 as needed to obtain multiple intermediate layers;
[0065] ③, prepare the upper green body by the same operation as step ①;
[0066] 4. Freezing and drying of slurry:
[0067] Place the mold in step 3 into a refrigerator and freeze it at -20℃ to -22℃ for 24h to 25h to ensure that the slurry is completely frozen. Then place the mold in a freeze dryer and freeze-dry for 72h to 74h to ensure that all ice crystals in the green body are sublimated to obtain a mullite thermal insulation material with an infrared reflection layer.
[0068] Specific implementation method 2: This implementation method is different from the specific implementation method 1 in that the drying temperature in step 1 is 80° C. and the drying time is 24 hours. The rest is the same as the specific implementation method 1.
[0069] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that all the binders in step 2 are silica sol. The rest is the same as specific implementation method 1 or 2.
[0070] Specific embodiment 4: This embodiment is different from specific embodiment 3 in that the preparation method of the silica sol described in step 2 is as follows:
[0071] Pour ethyl orthosilicate into a beaker, then pour in anhydrous ethanol and water to form a mixed solution, finally drop in dilute hydrochloric acid, stir evenly, then put the beaker into a water bath at 40℃~50℃ and keep warm for 1h to obtain silica sol;
[0072] The concentration of the dilute hydrochloric acid is 0.2 mol / L;
[0073] The molar ratio is ethyl orthosilicate: water: anhydrous ethanol: hydrogen chloride = 1:4:4:7.5×10 -4 . The rest is the same as the third specific implementation method.
[0074] Specific implementation mode 5: This implementation mode is different from specific implementation mode 4 in that the rotation speed of all stirring in step 2 is 1000 r / min. The rest is the same as specific implementation mode 4.
[0075] Specific implementation method 6: This implementation method is different from specific implementation method 5 in that the pressing sheet described in step 3① is an acrylic sheet. The rest is the same as specific implementation method 5.
[0076] Specific embodiment 7: This embodiment is different from specific embodiment 6 in that the tablet pressing described in step 3① is in close contact with the inner wall of the mold and is in sliding connection. The rest is the same as specific embodiment 6.
[0077] Specific embodiment 8: This embodiment is different from specific embodiment 7 in that the density of the mullite fiber in the lower green body described in step 3 is 0.23 g / cm 3 The density of mullite fiber in the upper green body is 0.23g / cm 3 The density of mullite fiber in the middle layer green body is 0.23g / cm 3 . The rest is the same as the specific implementation method seven.
[0078] Specific embodiment 9: This embodiment is different from specific embodiment 8 in that: in step 4, freezing at -20°C for 24 hours ensures that the slurry is completely frozen. The rest is the same as specific embodiment 8.
[0079] Specific embodiment 10: This embodiment differs from specific embodiment 9 in that the freeze-drying conditions in step 4 are: temperature of -50°C and vacuum degree of 50 Pa to 100 Pa. The rest is the same as specific embodiment 9.
[0080] The present invention is verified by the following tests:
[0081] Test 1: This test is a method for preparing a mullite thermal insulation material with an infrared reflection layer, which is specifically carried out in the following steps:
[0082] 1. Add the mullite fiber into deionized water, and then put it into the fiber beater for short-cutting. The short-cutting time is 20 minutes. After the short-cutting is completed, let it stand for 20 seconds. The fiber is retained from the liquid outlet at the bottom of the beater, and then filtered with gauze to leave only the fiber part, and then dried at a temperature of 80°C for 24 hours to obtain mullite short-cut fiber;
[0083] The bottom of the inner cavity of the fiber beater is horizontal;
[0084] The mass ratio of the mullite fiber to the deionized water is 1:100;
[0085] 2. Preparation of slurry:
[0086] ①, prepare the lower slurry: disperse the dried mullite chopped fibers in step 1 into the mixture of deionized water and binder, stir with a stirrer for 30 minutes to fully mix and form the lower slurry, and the stirring speed is 1000r / min;
[0087] The mass of the mullite chopped fibers is 1.5% of the mass of deionized water;
[0088] The mass of the binder is 5% of the mass of deionized water;
[0089] The binders are all silica sol, and the preparation method is as follows:
[0090] Pour ethyl orthosilicate into a beaker, then pour in anhydrous ethanol and water to form a mixed solution, finally drop in dilute hydrochloric acid, stir evenly, then put the beaker into a 45°C water bath and keep warm for 1 hour to obtain silica sol;
[0091] The concentration of the dilute hydrochloric acid is 0.2 mol / L;
[0092] The molar ratio is ethyl orthosilicate: water: anhydrous ethanol: hydrogen chloride = 1:4:4:7.5×10 -4 ;
[0093] The preparation method of the upper slurry is exactly the same as that of the lower slurry;
[0094] ②, prepare infrared reflective intermediate layer slurry: disperse the dried mullite chopped fibers and potassium hexatitanate whiskers in the step 1 into a mixture of deionized water and a binder, stir them with a stirrer for 30 minutes to fully mix them and form an infrared reflective intermediate layer slurry, and the stirring speed is 1000r / min;
[0095] The mass of the potassium hexatitanate whiskers is 9% of the mass of the mullite chopped fibers;
[0096] The mass of the mullite chopped fibers is 1.5% of the mass of deionized water;
[0097] The mass of the binder is 5% of the mass of deionized water;
[0098] The binders are all silica sol, and the preparation method is as follows:
[0099] Pour ethyl orthosilicate into a beaker, then pour in anhydrous ethanol and water to form a mixed solution, finally drop in dilute hydrochloric acid, stir evenly, then put the beaker into a 45°C water bath and keep warm for 1 hour to obtain silica sol;
[0100] The concentration of the dilute hydrochloric acid is 0.2 mol / L;
[0101] The molar ratio is ethyl orthosilicate: water: anhydrous ethanol: hydrogen chloride = 1:4:4:7.5×10 -4 ;
[0102] 3. ①. First, prepare the lower green body: pour the lower slurry prepared in step 2 into the mold, let it stand for 10 minutes, put a tablet wrapped with gauze on the upper part of the mold horizontally, apply pressure to the tablet vertically downward until the tablet moves downward to the target depth, and then continue to maintain pressure for 30 seconds. The excess water in the slurry flows to the top of the tablet through the through hole on the tablet, and then take out the water above the tablet (extracted by a syringe), and then take out the tablet to obtain the lower green body in the mold;
[0103] The surface of the pressing sheet is evenly provided with a plurality of through holes, the aperture of the through holes is 2.5 mm, the pressing sheet is an acrylic plate, and the pressing sheet is in close contact with the inner wall of the mold and is in sliding connection;
[0104] The density of the green body is controlled by controlling the pressing depth of the tablet;
[0105] ②Preparation of intermediate layer green body:
[0106] The intermediate layer slurry prepared in step 2 is slowly poured onto the top of the lower green sheet in the above-mentioned mold, and the whiskers are allowed to settle to the bottom after standing for 5 to 6 minutes. A pressing sheet wrapped with fine gauze is placed on the top of the mold, and pressure is applied vertically downward to the pressing sheet until the pressing sheet moves downward to the target depth, and then the pressure is maintained for 30 seconds. Excess water in the slurry flows to the top of the pressing sheet through the through hole on the pressing sheet, and then the water on the pressing sheet is taken out, and then the pressing sheet is taken out to obtain the intermediate layer green sheet in the mold. The bottom of the intermediate layer green sheet is the infrared reflection layer where the potassium hexatitanate whiskers are concentratedly distributed, and a small amount of whiskers will adhere to the mullite fiber mesh structure during the sedimentation process;
[0107] ③, prepare the upper green body by the same operation as step ①;
[0108] The density of the mullite fiber in the lower green body described in step 3 is 0.23 g / cm 3 The density of mullite fiber in the upper green body is 0.23g / cm 3 The density of mullite fiber in the middle layer green body is 0.23g / cm 3 ; Density is obtained by dividing the mass of mullite chopped fibers in the corresponding layer by the volume of the corresponding layer;
[0109] 4. Freezing and drying of slurry:
[0110] Place the mold in step three in a refrigerator and freeze it at -20°C for 24 hours to ensure that the slurry is completely frozen. Then place the mold in a freeze dryer and freeze-dry for 72 to 74 hours to ensure that all ice crystals in the green body are sublimated to obtain a mullite insulation material with an infrared reflection layer. The freeze-drying conditions are: temperature of -50°C and vacuum of 50Pa.
[0111] Figure 1 This is a top view photo of the mullite thermal insulation material with an infrared reflection layer prepared for Test 1. The sample is in the shape of a white disk with a diameter of about 20 cm.
[0112] Figure 2 This is a front view photo of the mullite thermal insulation material with an infrared reflection layer prepared in Experiment 1. It can be seen that the sample is about 2 cm thick and is divided into a lower layer, a middle layer and an upper layer. The thickness of the lower and upper layers is about 5 mm, and they are composed of mullite fiber blanks, and the color is bright white; the middle layer is the area between the two yellow lines, and the thickness of the middle layer is about 10 mm. It is composed of mullite fibers and potassium hexatitanate whiskers, and the color is slightly yellow. The bottom of the middle layer is an infrared reflection layer with concentrated distribution of potassium hexatitanate whiskers.
[0113] Figure 3 This is a schematic diagram of the infrared reflective intermediate layer slurry prepared in step 2 of the present invention, in which potassium hexatitanate whiskers and mullite fibers are uniformly mixed.
[0114] Figure 4 This is a schematic diagram of the pressed sheet after the intermediate layer green body is prepared in step 3, where the bottom is the potassium hexatitanate crystal system infrared reflection layer, and the top is mainly mullite fiber. The mullite fiber settles to form a three-dimensional network structure. Since the potassium hexatitanate whisker settles faster than the mullite fiber, most of the coarse whiskers will form an infrared reflection layer near the hot surface at the bottom where the whiskers are concentrated after standing. Due to the existence of the mullite fiber network, a small amount of fine whiskers will still be attached to the fiber.
[0115] Figure 5 This is a schematic diagram of the case where multiple reflective layers are required when preparing the intermediate layer green body in step 3. The number of layers of the infrared reflective layer can be adjusted by adjusting the number of times the intermediate layer slurry is poured into the mold in batches, and the thickness of the infrared reflective layer can be controlled by adjusting the amount of slurry poured each time and the content of whiskers in the slurry. The layered design and optimization of materials can be achieved through process control.
[0116] Figure 6 This is the SEM image of the potassium hexatitanate whiskers used in step 2 of experiment 1. It can be seen that the distribution of whisker diameters varies greatly. The content of fine whiskers is relatively small, with a diameter of about 1 to 5 μm, and relatively good dispersion. They are easy to adhere to the mullite fiber during the sedimentation process. The content of coarse whiskers is relatively large, with a diameter of about 10 to 50 μm, poor dispersion, and they are easy to quickly settle to form an infrared reflection layer.
[0117] Figure 7 The SEM image of the upper layer of the mullite thermal insulation material with infrared reflection layer prepared for test 1 shows that the diameter of the mullite fiber is about 1 to 10 μm. The sample is made of overlapping fibers, and the overlapping is disordered and random, forming a three-dimensional network-like spatial structure, which is a high-porosity thermal insulation material.
[0118] Figure 8 The SEM image of the middle layer of the mullite thermal insulation material with an infrared reflection layer prepared for Test 1 shows that it is composed of a mullite fiber network structure and potassium hexatitanate whiskers filled therein, most of which are relatively thin.
[0119] Experiment 2: This experiment is different from Experiment 1 in that the mass of the potassium hexatitanate whiskers described in step 2② is 0.0 of the mass of the mullite chopped fibers. The rest is the same as Experiment 1.
[0120] Experiment 3: This experiment is different from Experiment 1 in that the mass of the potassium hexatitanate whiskers described in step 2② is 18% of the mass of the mullite chopped fibers. The rest is the same as Experiment 1.
[0121] Experiment 4: This experiment is different from Experiment 1 in that the mass of the potassium hexatitanate whiskers described in step 2② is 27% of the mass of the mullite chopped fibers. The rest is the same as Experiment 1.
[0122] Experiment 5: This experiment is different from Experiment 1 in that the mass of the potassium hexatitanate whiskers described in step 2② is 36% of the mass of the mullite chopped fibers. The rest is the same as Experiment 1.
[0123] Fig. 9 This is a graph showing the relationship between the potassium hexatitanate whisker content and thermal conductivity in the mullite thermal insulation material with an infrared reflection layer prepared in experiments 1 to 5. The green curve corresponds to a test temperature of 1200°C, and the orange line corresponds to a test temperature of 800°C. The number of infrared reflection layers in this group of samples is 1. As can be seen from the figure, when potassium hexatitanate whiskers are not added (experiment 2), the thermal conductivity of the material at 1200°C is 0.122W / (m·K), but when the whisker content is 9% (experiment 1) and 18% (experiment 3), the high-temperature thermal conductivity increases. This is because the whisker content is small, and most of the whiskers are retained in the three-dimensional network of mullite fibers during the sedimentation process, which increases the material density, while the infrared reflection layer formed by a small amount of whiskers that settle to the bottom is too thin, resulting in an increase in thermal conductivity. When the whisker content is 27% (Test 4), the thermal conductivity at 1200°C is 0.106W / (m·K). This is because the whiskers settle to form an infrared reflection layer where the whiskers are concentrated, which significantly inhibits heat transfer at high temperatures. When the whisker content is 36% (Test 5), the thermal conductivity at 1200°C is 0.109W / (m·K). The infrared reflection layer still exists, but the excess whiskers are retained on the three-dimensional network of mullite fibers, which increases the material density, so the high-temperature thermal conductivity increases slightly. The trend of thermal conductivity change at 800°C is similar. Therefore, the optimal content of potassium hexatitanate whiskers is 27%.
[0124] Test 6: This test is different from Test 4 in that in step 3②, the intermediate layer slurry is evenly poured into the mold three times, and after each addition of the intermediate layer slurry, a tablet pressing and drainage process (the same as Test 4) is required to obtain three intermediate infrared reflective layers. The rest is the same as Test 4.
[0125] Fig.10 This is a graph showing the relationship between the number of infrared reflection layers and thermal conductivity in the mullite thermal insulation material with infrared reflection layers prepared in Experiments 4 and 6. It can be seen that as the number of infrared reflection layers increases from 1 layer (Experiment 4) to 3 layers (Experiment 6), the thermal conductivity of the material at 1200°C decreases from 0.106W / (m·K) to 0.103W / (m·K), and the thermal conductivity at 800°C decreases from 0.074W / (m·K) to 0.072W / (m·K). This is because although the total amount of potassium hexatitanate whiskers remains unchanged, the whisker distribution is optimized through the layer-by-layer sedimentation molding process; although the thickness of the single-layer reflection layer becomes thinner, the number of reflection layers increases, providing the sample with the ability of multiple reflections. When the total amount of infrared reflective agent is the same, the multiple reflection effect is better than the single reflection.
[0126] The thermal conductivity test methods used in the present invention are all YBT 4130-2005 refractory thermal conductivity test method (water flow plate method).
Claims
1. A method for preparing a mullite thermal insulation material having an infrared reflection layer, characterized in that The preparation method of the mullite thermal insulation material with an infrared reflection layer is carried out according to the following steps:
1. Add the mullite fiber into deionized water, and then put it into the fiber beater for short-cutting. The short-cutting time is 20min-25min. After the short-cutting is completed, let it stand for 20s-25s. The fiber is retained from the liquid outlet at the bottom of the beater, and then filtered with gauze to leave only the fiber part, and then dried to obtain mullite short-cut fiber; The bottom of the inner cavity of the fiber beater is horizontal; The mass ratio of the mullite fiber to the deionized water is 1:(100-110); 2. Preparation of slurry: ①, prepare the lower slurry: disperse the dried mullite chopped fibers in step 1 into the mixed solution of deionized water and binder, and stir with a stirrer for 30min to 35min to fully mix and evenly form the lower slurry; The mass of the mullite chopped fibers is 1.5% to 2% of the mass of deionized water; The mass of the binder is 5% to 5.5% of the mass of deionized water; The preparation method of the upper slurry is exactly the same as that of the lower slurry; ②, prepare infrared reflective intermediate layer slurry: disperse the dried mullite chopped fibers and potassium hexatitanate whiskers in a mixture of deionized water and a binder, and stir them with a stirrer for 30 to 35 minutes to fully mix them to form an infrared reflective intermediate layer slurry; The mass of the potassium hexatitanate whiskers is 9% to 36% of the mass of the mullite chopped fibers; The mass of the mullite chopped fibers is 1.5% to 2% of the mass of deionized water; The mass of the binder is 5% to 5.5% of the mass of deionized water; 3. ①. First, prepare the lower green sheet: pour the lower slurry prepared in step 2 into the mold, let it stand for 10 to 15 minutes, put a pressing sheet wrapped with fine gauze on the upper part of the mold horizontally, apply pressure to the pressing sheet vertically downward until the pressing sheet moves downward to the target depth, and then continue to maintain the pressure for 30 to 35 seconds. The excess water in the slurry flows to the top of the pressing sheet through the through hole on the pressing sheet, and then the water on the pressing sheet is taken out, and then the pressing sheet is taken out to obtain the lower green sheet in the mold; The surface of the tablet is evenly provided with a plurality of through holes, and the diameter of the through holes is 2.5 mm to 3 mm; The density of the green body is controlled by controlling the pressing depth of the tablet; ②Preparation of intermediate layer green body: a. Slowly pour the intermediate layer slurry prepared in step 2 onto the top of the lower green sheet in the above-mentioned mold, let it stand for 5-6 minutes until the whiskers settle to the bottom, put a pressing sheet wrapped with fine gauze on the top of the mold, apply pressure vertically downward to the pressing sheet until the pressing sheet moves downward to the target depth, and then continue to maintain the pressure for 30-35 seconds, and the excess water in the slurry flows to the top of the pressing sheet through the through hole on the pressing sheet, and then the water on the pressing sheet is taken out, and then the pressing sheet is taken out to obtain the intermediate layer green sheet in the mold, the bottom of the intermediate layer green sheet is the infrared reflection layer where the potassium hexatitanate whiskers are concentratedly distributed, and a small amount of whiskers will adhere to the mullite fiber mesh structure during the sedimentation process; b. Repeat step 1 as needed to obtain multiple intermediate layers; ③, prepare the upper green body by the same operation as step ①; 4. Freezing and drying of slurry: Place the mold in step 3 into a refrigerator and freeze it at -20℃ to -22℃ for 24h to 25h to ensure that the slurry is completely frozen. Then place the mold in a freeze dryer and freeze-dry for 72h to 74h to ensure that all ice crystals in the green body are sublimated to obtain a mullite thermal insulation material with an infrared reflection layer.
2. The method for preparing a mullite thermal insulation material having an infrared reflection layer according to claim 1, characterized in that The drying temperature in step 1 is 80° C. and the drying time is 24 hours.
3. The method for preparing a mullite thermal insulation material having an infrared reflection layer according to claim 1, characterized in that All the binders in step 2 are silica sol, and the preparation method of silica sol is as follows: Pour ethyl orthosilicate into a beaker, then pour in anhydrous ethanol and water to form a mixed solution, finally drop in dilute hydrochloric acid, stir evenly, then put the beaker into a water bath at 40℃~50℃ and keep warm for 1h to obtain silica sol; The concentration of the dilute hydrochloric acid is 0.2 mol / L; The molar ratio is ethyl orthosilicate: water: anhydrous ethanol: hydrogen chloride = 1:4:4:7.5×10 -4 .
4. The method for preparing a mullite thermal insulation material having an infrared reflection layer according to claim 1, characterized in that When preparing the upper green body in step 2, silicon oxide aerogel, a material with lower thermal conductivity, can be introduced to further reduce the heat transfer of the upper layer.
5. The method for preparing a mullite thermal insulation material having an infrared reflection layer according to claim 1, characterized in that The rotation speed of all stirring in step 2 is 1000r / min.
6. The method for preparing a mullite thermal insulation material having an infrared reflection layer according to claim 1, characterized in that The pressing sheet described in step 3① is an acrylic sheet.
7. The method for preparing a mullite thermal insulation material having an infrared reflection layer according to claim 1, characterized in that The pressing tablet described in step 3① is in close contact with the inner wall of the mold and is slidably connected.
8. The method for preparing a mullite thermal insulation material having an infrared reflection layer according to claim 1, characterized in that The density of the mullite fiber in the lower green body described in step 3 is 0.23 g / cm 3 The density of mullite fiber in the upper green body is 0.23g / cm 3 The density of mullite fiber in the middle layer green body is 0.23g / cm 3 .
9. The method for preparing a mullite thermal insulation material having an infrared reflection layer according to claim 1, characterized in that In step 4, the slurry is frozen at -20°C for 24 hours to ensure that the slurry is completely frozen.
10. The method for preparing a mullite thermal insulation material having an infrared reflection layer according to claim 9, characterized in that The freeze-drying conditions in step 4 are: temperature of -50°C and vacuum degree of 50Pa to 100Pa.