Doped iron-based nanocrystalline powder ferrite magnetic material and preparation method thereof
Through the combination of iron-based nanocrystal powder and iron oxide and other elements and low-temperature sintering technology, the problem of high-temperature sintering in the preparation of traditional soft ferrite materials is solved, and the permeability and pressure resistance are improved. It is suitable for high-frequency application.
Patent Information
- Application Number
- CN202410894571.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional soft ferrite materials require high temperature sintering during the preparation process, resulting in high energy loss and production costs, and poor permeability and pressure resistance.
Doped iron-based nanocrystal powder is used to form an amorphous alloy through rapid cooling, and annealing is carried out to form nanocrystals, and pre-sintering, ball milling, granulation and pressing are combined with iron oxide, zinc oxide, magnesium oxide and other elements for pre-sintering, ball milling, granulation and pressing, and finally at a lower level Sintered at temperature to prepare ferrite magnetic materials with high permeability and pressure resistance.
It is realized that ferrite magnetic materials with high permeability and good pressure resistance are prepared at lower sintering temperatures, and are suitable for use in the high frequency range of 1MHz-100MHz, reducing production costs and energy consumption.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnetic materials, and in particular relates to an iron-based nanocrystalline powder doped ferrite magnetic material and a preparation method thereof. Background Art
[0002] Ferrites are composite oxides composed of iron oxide and one or more other metal oxides. Ferrite with ferrimagnetism is a strong magnetic material, commonly known as ferrite magnetic material. Ferrite magnetic materials can be divided into soft magnetic, hard magnetic (including bonding), gyromagnetic, moment magnetic, piezomagnetic and other ferrite materials. Their main characteristics are: soft magnetic materials have high magnetic permeability, low coercive force and low loss; hard magnetic materials have high coercive force Hc and high magnetic energy product (BH)m; gyromagnetic materials have gyromagnetic characteristics, that is, when electromagnetic waves propagate along the direction of a constant magnetic field, their vibration surface rotates continuously along the propagation direction. Gyromagnetic materials are mainly used in microwave communication devices. Moment magnetic materials have a rectangular B-H hysteresis loop and are mainly used in computer storage cores; piezomagnetic materials have a large linear magnetostriction coefficient λs. Ferrite magnetic materials have been widely used in the fields of computers, microwave communications, televisions, automatic control, aerospace, instrumentation, medical treatment, and automobile industries, among which hard and soft ferrite materials are the most widely used.
[0003] Traditional soft ferrite materials require high-temperature sintering during the preparation process, which increases energy loss and production costs. In addition, the prepared soft ferrite materials cannot improve the magnetic permeability of ferrite materials and have poor pressure resistance. Summary of the invention
[0004] The purpose of the present invention is to provide an iron-doped nanocrystalline powder ferrite magnetic material and a preparation method thereof in order to solve the above problems.
[0005] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0006] A doped iron-based nanocrystalline powder ferrite magnetic material is prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 1-6 parts of iron-based nanocrystalline powder;
[0007] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0008] As one embodiment thereof: prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, 1 part of iron-based nanocrystalline powder;
[0009] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0010] As one embodiment thereof: prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 2 parts of iron-based nanocrystalline powder;
[0011] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0012] As one embodiment thereof: prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, 3 parts of iron-based nanocrystalline powder;
[0013] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0014] As one embodiment thereof: prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, 3.5 parts of iron-based nanocrystalline powder;
[0015] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0016] As one embodiment thereof: prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, 4 parts of iron-based nanocrystalline powder;
[0017] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0018] As one embodiment thereof: prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, 5 parts of iron-based nanocrystalline powder;
[0019] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0020] As one embodiment thereof: prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, 6 parts of iron-based nanocrystalline powder;
[0021] The atomic percentage of each element in the iron-based nanocrystalline powder is 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe
[0022] The present invention also provides a method for preparing an iron-doped nanocrystalline powder ferrite magnetic material, comprising the following steps:
[0023] Step 1: After preparing the master alloy using industrial raw materials, the amorphous alloy strip is formed by rapid cooling, and nanocrystals are formed by annealing, and then ground into iron-based nanocrystal powder;
[0024] Step 2: Weigh and mix iron oxide, zinc oxide, magnesium oxide, nickel oxide, manganese oxide, copper oxide, bismuth oxide, silicon oxide, vanadium oxide, and aluminum oxide according to the formula, and add iron-based nanocrystalline powder;
[0025] Step 3: pre-sintering, ball milling, granulation and pressing the prepared mixture to form a blank;
[0026] Step 4: Sintering the blank to obtain iron-doped nanocrystalline powder ferrite magnetic material.
[0027] The sintering temperature is 1155°C-1180°C.
[0028] The advantages are as follows:
[0029] 1. By selecting the specific composition and weight proportion of each component, a relatively low sintering temperature (not exceeding 1200° C.) can be used during the sintering process to obtain a ferrite material.
[0030] 2. The obtained ferrite material has high magnetic permeability (inductance value) and withstand voltage (anti-puncture capability), and can meet the use in the high frequency range of 1MHz-100MHz. DETAILED DESCRIPTION
[0031] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to these embodiments.
[0032] Example 1
[0033] A doped iron-based nanocrystalline powder ferrite magnetic material is prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 1 part of iron-based nanocrystalline powder;
[0034] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0035] Example 2
[0036] A doped iron-based nanocrystalline powder ferrite magnetic material is prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 2 parts of iron-based nanocrystalline powder;
[0037] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0038] Example 3
[0039] A doped iron-based nanocrystalline powder ferrite magnetic material is prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 3 parts of iron-based nanocrystalline powder;
[0040] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0041] Example 4
[0042] A doped iron-based nanocrystalline powder ferrite magnetic material is prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 3.5 parts of iron-based nanocrystalline powder;
[0043] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0044] Example 5
[0045] A doped iron-based nanocrystalline powder ferrite magnetic material is prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 4 parts of iron-based nanocrystalline powder;
[0046] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0047] Example 6
[0048] A doped iron-based nanocrystalline powder ferrite magnetic material is prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 5 parts of iron-based nanocrystalline powder;
[0049] The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0050] Example 7
[0051] A doped iron-based nanocrystalline powder ferrite magnetic material is prepared from the following raw materials by mass: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 6 parts of iron-based nanocrystalline powder;
[0052] The atomic percentage of each element in the iron-based nanocrystalline powder is 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
[0053] Test conditions:
[0054] Core size Φ6×8mm, 176 turns of winding;
[0055] Test frequency and voltage: 1kHz / 0.25V;
[0056] Test temperature: room temperature 25℃;
[0057] Undoped: inductance L=1300uH, withstand voltage 2500V;
[0058] Example 1 doped with 1 part of Fe-B-Si-Nb-Cu iron-based nanocrystalline powder: inductance value L=1330uH, withstand voltage 2800V;
[0059] Example 2 doped with 2 parts of Fe-B-Si-Nb-Cu iron-based nanocrystalline powder: inductance value L=1380uH, withstand voltage 3500V;
[0060] Example 3 doping 3 parts of Fe-B-Si-Nb-Cu iron-based nanocrystalline powder: inductance value L=1480uH, withstand voltage 4500V;
[0061] Example 4 doped with 3.5 parts of Fe-B-Si-Nb-Cu iron-based nanocrystalline powder: inductance value L=1500uH, withstand voltage 4550V;
[0062] Example 5 doped with 4.0 parts of Fe-B-Si-Nb-Cu iron-based nanocrystalline powder: inductance value L=1520uH, withstand voltage 4560V;
[0063] Example 6 doping 5 parts of Fe-B-Si-Nb-Cu iron-based nanocrystalline powder: inductance value L=1510uH, withstand voltage 4550V;
[0064] Example 7 doped with 6 parts of Fe-B-Si-Nb-Cu iron-based nanocrystalline powder: inductance value L=1520uH, withstand voltage 4500V.
[0065] The present invention also provides a method for preparing an iron-doped nanocrystalline powder ferrite magnetic material, comprising the following steps:
[0066] Step 1: After preparing the master alloy using industrial raw materials, the amorphous alloy strip is formed by rapid cooling, and nanocrystals are formed by annealing, and then ground into iron-based nanocrystal powder;
[0067] Step 2: Weigh and mix iron oxide, zinc oxide, magnesium oxide, nickel oxide, manganese oxide, copper oxide, bismuth oxide, silicon oxide, vanadium oxide, and aluminum oxide according to the formula, and add iron-based nanocrystalline powder;
[0068] Step 3: pre-sintering, ball milling, granulation and pressing the prepared mixture to form a blank;
[0069] Step 4: Sintering the blank to obtain iron-doped nanocrystalline powder ferrite magnetic material.
[0070] The sintering temperature is 1155°C-1180°C.
[0071] The above-mentioned embodiments only express the implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A doped iron-based nanocrystalline powder ferrite magnetic material, characterized in that: The invention is prepared from raw materials of the following mass components: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 1-6 parts of iron-based nanocrystalline powder; The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
2. The iron-doped nanocrystalline powder ferrite magnetic material according to claim 1, characterized in that: The invention is prepared from the following raw materials by weight: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 1 part of iron-based nanocrystalline powder; The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
3. The iron-doped nanocrystalline powder ferrite magnetic material according to claim 1, characterized in that: The invention is prepared from the following raw materials by weight: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 2 parts of iron-based nanocrystalline powder; The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
4. The iron-doped nanocrystalline powder ferrite magnetic material according to claim 1, characterized in that: The invention is prepared from the following raw materials by weight: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 3 parts of iron-based nanocrystalline powder; The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
5. The iron-doped nanocrystalline powder ferrite magnetic material according to claim 1, characterized in that: The invention is prepared from raw materials of the following mass components: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 3.5 parts of iron-based nanocrystalline powder; The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
6. The iron-doped nanocrystalline powder ferrite magnetic material according to claim 1, characterized in that: The invention is prepared from the following raw materials by weight: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 4 parts of iron-based nanocrystalline powder; The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
7. The iron-doped nanocrystalline powder ferrite magnetic material according to claim 1, characterized in that: The invention is prepared from the following raw materials by weight: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 5 parts of iron-based nanocrystalline powder; The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
8. The iron-doped nanocrystalline powder ferrite magnetic material according to claim 1, characterized in that: The invention is prepared from the following raw materials by weight: 60-65 parts of iron oxide, 10.5-13 parts of zinc oxide, 8-15 parts of magnesium oxide, 1-5 parts of nickel oxide, 1.5-4 parts of manganese oxide, 1.6-3.5 parts of copper oxide, 0.8-1.7 parts of bismuth oxide, 0.5-1.2 parts of silicon oxide, 0.5-1.2 parts of vanadium oxide, 0.5-1.2 parts of aluminum oxide, and 5 parts of iron-based nanocrystalline powder; The atomic percentages of the elements in the iron-based nanocrystalline powder are 6%-10% Si, 5%-10% B, 1%-6% P, 0.5%-2% Nb, 0.5%-1.5% Cu, and the balance is Fe.
9. The method for preparing a doped iron-based nanocrystalline powder ferrite magnetic material according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: After preparing the master alloy using industrial raw materials, the amorphous alloy strip is formed by rapid cooling, and nanocrystals are formed by annealing, and then ground into iron-based nanocrystal powder; Step 2: Weigh and mix iron oxide, zinc oxide, magnesium oxide, nickel oxide, manganese oxide, copper oxide, bismuth oxide, silicon oxide, vanadium oxide, and aluminum oxide according to the formula, and add iron-based nanocrystalline powder; Step 3: pre-sintering, ball milling, granulation and pressing the prepared mixture to form a blank; Step 4: Sintering the blank to obtain iron-doped nanocrystalline powder ferrite magnetic material.
10. The method for preparing a doped iron-based nanocrystalline powder ferrite magnetic material according to claim 9, characterized in that: The temperature of the sintering treatment is 1155°C-1180°C.
Citation Information
Patent Citations
High saturation magnetization intensity Fe-based nanocrystalline magnetically soft alloy material and preparation method thereof
CN101834046A
Nano-iron powder-containing soft magnetic ferrite materials and preparation method
CN104900367A
Preparation method for iron-based nanocrystalline magnetic powder core
CN105810383A
Magnet having regions of different magnetic properties and method for forming such a magnet
CN106796835A
Ferrite material and preparation method thereof
CN110204325A