A-site and B-site double-doped medium-entropy lead zirconate-based composite dielectric ceramic and preparation method thereof
By performing the A and B-position dual doping in the B-position lattice of lead zirconate and adding PbSnO3, the problem of improving the dielectric performance of lead zirconate is solved, and the dielectric constant is improved and the dielectric constant is improved. The loss is reduced and the process is simple and efficient.
Patent Information
- Application Number
- CN202411005189.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-25
AI Technical Summary
In the field of dielectric ceramics, no intermediate entropy design and complex phase research or reports have been conducted on A and B positions double doping lead zirconate, resulting in the failure to fully improve its dielectric performance.
By doping three elements with similar chemical properties in the B-position lattice of lead zirconate in equal molar ratio and partially entropy design at the A-position, it causes lattice distortion and increases the degree of chaos. A small amount of PbSnO3 is added to design the complex phase Ceramics, improve dielectric properties. Specific methods include preparing ceramics according to the chemical formula xPbSnO3-(1-x)(Pb0.96La0.01Ba0.01Sm0.01)(Hf1/3Zr1/3Ti1/3)O3, using three-dimensional mixing, pre-firing, wet ball milling, drying, Grinding, tableting and sintering.
The dielectric constant is increased and the dielectric loss is reduced. The process is simple and there is no need to add binder or sintering aid. The sintering time is short, energy saving, short production cycle and high efficiency.
Smart Images

Figure CN118908727A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an A- and B-site dual-doped medium-entropy lead zirconate-based multiphase dielectric ceramic and a preparation method thereof, belonging to the technical field of medium-entropy ceramics. Background Art
[0002] Lead zirconate (PbZrO3) is a typical dielectric ceramic material. After doping, the dielectric constant can be increased and the dielectric loss can be reduced.
[0003] Medium entropy ceramic materials are multi-principal solid solution ceramics formed by doping 3 to 4 elements in equal or approximately equal proportions. In the field of dielectric ceramics, there has never been a study or report on the design of dual doping and medium entropy treatment of lead zirconate at A and B positions and complex phase. This patent is to design dual doping and medium entropy treatment of lead zirconate at A and B positions, and dope three elements with similar chemical properties in equal molar ratios into the B-position lattice of lead zirconate, and at the same time perform partial medium entropy treatment at the A position, so that it can ensure that the A position contains a large amount of Pb elements, and after partial medium entropy treatment, the disorder of the A position will increase. After dual doping and medium entropy treatment of A and B positions, the lead zirconate can produce a lattice distortion effect, which increases its disorder. Adding a small amount of PbSnO3 for complex phase ceramic design is expected to further improve the dielectric properties. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing an A- and B-doped mid-entropy lead zirconate-based composite dielectric ceramic, the chemical formula of which is: xPbSnO 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, (x = 0 to 0.03). The preparation method comprises the following steps:
[0005] (1) According to (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, weigh BaCO3, La2O3, Sm2O3, HfO2, ZrO2, and TiO2 powders respectively; weigh SnO2 and PbO powders respectively according to the chemical formula of PbSnO3.
[0006] (2) The above powders were placed in a three-dimensional mixer for mixing for 30 to 50 minutes, and then pre-calcined. The pre-calcined powders were divided into xPbSnO 3-(1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 (x = 0 ~ 0.03) chemical formula weigh PbSnO3 and (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, respectively put them into a ball mill for wet ball milling, and then grind, sieve and tablet press after drying;
[0007] (3) The pressed unsintered ceramic sheet is placed in a muffle furnace and sintered at 1200-1270°C in air.
[0008] Preferably, in step (2), the pre-burning (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 The pre-sintering temperature of )O3 medium entropy ceramic powder is 800~850℃, and the holding time is 1.8~2.2h. The pre-sintering temperature of PbSnO3 ceramic powder is 800~850℃, and the holding time is 1.7~2.3h.
[0009] Preferably, the conditions for wet ball milling in step (2) are: the rotation speed of the ball mill is 15 to 35 rpm, the ball milling time is 36 to 72 hours, the ball milling medium is distilled water and zirconia balls, the mass ratio of zirconia balls: material to be ground: distilled water is 0.9:3:1; the mass ratio of large balls, medium balls, and small balls in the zirconia balls is 1:2:3.
[0010] Preferably, the drying conditions in step (2) are as follows: the drying temperature in step (2) is 80 to 120° C., and the drying time is 12 to 20 hours.
[0011] Preferably, the mesh size of the sieve in step (2) is 80 to 200 meshes.
[0012] Preferably, the grinding conditions in step (2) are: placing the dried mixed powder into a grinding jar and grinding for 20 to 50 minutes.
[0013] Preferably, the diameter of the mold used for tableting in step (2) is 10 to 13 mm, the uniaxial pressure is 160 to 180 MPa, and the holding time is 5 to 15 minutes.
[0014] Preferably, the sintering method in step (3) is: adding the same powder as the ceramic sheet around and on the top of the ceramic sheet for burying and burning, raising the temperature of the muffle furnace from room temperature to 1200-1270°C at a heating rate of 4.5°C / min, keeping the temperature in the muffle furnace for 2.8-3.2 hours, and then taking it out after cooling to a low temperature with the furnace.
[0015] The beneficial effects of the present invention are:
[0016] (1) The preparation process of the present invention is simple and does not require atmosphere protection. It only needs to use an ordinary muffle furnace for sintering, which has the characteristics of short sintering time, energy saving, simple process, low production cost, short production cycle, high efficiency, etc.
[0017] (2) xPbSnO prepared by the present invention 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, (x=0~0.03) composite medium entropy ceramics do not require the addition of any binder, sintering aid and dispersant.
[0018] (3) xPbSnO prepared by the present invention 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, (x=0-0.03). The dielectric constant of the medium entropy ceramics is 825 at room temperature under a 1kHz frequency test, and the dielectric loss is less than 0.05. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The xPbSnO prepared in Examples 1 to 3 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, (x=0~0.03) XRD of composite medium-entropy ceramics.
[0020] Figure 2 The (Pb 0.96 La0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 ) SEM image of O3 mesoentropic ceramics;
[0021] Figure 3 The xPbSnO prepared in Examples 1 to 3 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, (x=0~0.03) dielectric constant diagram of the entropy ceramics in the composite phase at room temperature.
[0022] Figure 4 The xPbSnO prepared in Examples 1 to 3 3- (1-x)(Pb 0.93 La 0.02 Ba 0.02 Sm 0.02 )(Sn 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, (x=0~0.03) room temperature dielectric loss diagram of the complex phase mesoentropy ceramics. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further described below in conjunction with the accompanying drawings. However, the protection scope of the present invention is not limited to the above contents.
[0024] Example 1
[0025] The chemical formula of an A- and B-site dual-doped mid-entropy lead zirconate-based composite dielectric ceramic is: xPbSnO 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3.
[0026] In this embodiment, x=0, that is, (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3.
[0027] The preparation method of the above dielectric ceramic is as follows:
[0028] (1) PbO, BaCO3, La2O3, Sm2O3, HfO2, ZrO2, and TiO2 powders were weighed according to the stoichiometric ratio designed by the chemical formula. The above powders were placed in a three-dimensional mixer for mixing for 35 minutes, and then the mixed powders were pre-burned at a temperature of 850°C for 1.9 hours. The pre-burned powders were placed in a ball mill for wet ball milling. The speed of the ball mill was 28 rpm, and the ball milling time was 36 hours. The ball milling media were distilled water and zirconia balls. The mass ratio of zirconia balls: the material to be ground: distilled water was 3:1:0.9. The mass ratio of large balls, medium balls, and small balls in zirconia balls was 1:2:3. Then the mixture was dried at a temperature of 94°C for 16 hours. The dried mixed powder was placed in a grinding jar and ground for 31 minutes. The ground mixed powder was sieved with a mesh size of 180 meshes. The sieved mixed medium entropy powder was tableted. The mold diameter used for tableting was 13 mm, the uniaxial pressure was 180 MPa, and the holding time was 10 minutes.
[0029] (2) The pressed unsintered ceramic sheet is placed in a muffle furnace and sintered at 1235°C in air. The specific method is as follows: the same powder as the ceramic block is added around and on the ceramic block for burial firing, and the temperature of the muffle furnace is increased from room temperature to 1235°C at a heating rate of 4.5°C / min. The muffle furnace is kept warm for 3 hours, and then the ceramic sheet is taken out after cooling to a low temperature.
[0030] Example 2
[0031] The chemical formula of an A- and B-site dual-doped mid-entropy lead zirconate-based composite dielectric ceramic is: xPbSnO 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3. In this embodiment, x=0.015, i.e. 0.015PbSnO 3- 0.985(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3.
[0032] (1) According to (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01)(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3's chemical formula: Weigh BaCO3, La2O3, Sm2O3, HfO2, ZrO2, and TiO2 powders respectively. Put the above powders into a three-dimensional mixer for mixing for 38 minutes, and pre-sinter the mixed powders for 1.9 hours at a temperature of 845°C; put the pre-sintered powders into a ball mill for wet ball milling mixing. The speed of the ball mill is 30 rpm, the ball milling time is 34 hours, the ball milling medium is distilled water and zirconia balls, and the mass ratio of zirconia balls: the material to be ground: distilled water is 3:1:0.9. The mass ratio of large balls, medium balls, and small balls in zirconia balls is 1:2:3. Then dry them at a temperature of 94°C and a drying time of 16 hours. Put the dried mixed powder into a grinding jar for grinding for 31 minutes, sieve the ground mixed powder, the mesh number of the sieve is 180, and obtain (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 powder.
[0033] (2) Weigh SnO2 and PbO powders according to the chemical formula of PbSnO3. Pre-calculate SnO2 and PbO powders for 2 hours at a temperature of 840°C. Place the pre-calculated powders in a ball mill for wet milling. The speed of the ball mill is 30 rpm. The milling time is 34 hours. The milling media are distilled water and zirconia balls. The mass ratio of zirconia balls: material to be ground: distilled water is 3:1:0.9. The mass ratio of large balls, medium balls, and small balls in zirconia balls is 1:2:3. Dry the mixture at a temperature of 95°C and a drying time of 17 hours. Place the dried mixed powder in a grinding jar for grinding for 30 minutes. Sieve the ground mixed powder with a mesh size of 180 to obtain PbSnO3 powder.
[0034] (3) The pre-burned powder is treated as follows:
[0035] 0.015PbSnO 3- 0.985(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 chemical formula weigh PbSnO3 and (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01)(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 powder, put the mixed powder into a ball mill for wet ball milling, the speed of the ball mill is 29 rpm, the ball milling time is 38 hours, the ball milling medium is distilled water and zirconia balls, and the mass ratio of zirconia balls: material to be ground: distilled water is 3:1:0.9. The mass ratio of large balls, medium balls and small balls in zirconia balls is 1:2:3. Then dry, the drying temperature is 92°C, and the drying time is 17h. Put the dried mixed powder into a grinding jar for grinding for 31 minutes, sieve the ground mixed powder, the mesh number of the sieve is 150 mesh, and press the sieved mixed medium entropy powder into tablets. The diameter of the mold used for tableting is 13mm, the uniaxial pressure is 178MPa, and the holding time is 11 minutes.
[0036] (4) The pressed unsintered ceramic sheet is placed in a muffle furnace and sintered at 1250°C in air. The same powder as the ceramic sheet is added around and on the top of the ceramic sheet for burial firing. The temperature of the muffle furnace is raised from room temperature to 1250°C at a heating rate of 4.5°C / min. The temperature is kept in the muffle furnace for 3.1 hours, and then the muffle furnace is cooled to a low temperature and taken out.
[0037] Example 3
[0038] The chemical formula of an A- and B-site dual-doped mid-entropy lead zirconate-based composite dielectric ceramic is: xPbSnO 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3. In this embodiment, x=0.03, i.e., 0.03PbSnO3-0.97(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3.
[0039] (1) According to (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3)O3's chemical formula: Weigh BaCO3, La2O3, Sm2O3, HfO2, ZrO2, and TiO2 powders respectively. Put the above powders into a three-dimensional mixer for mixing for 43 minutes, pre-sinter the mixed powders for 1.9 hours at a temperature of 843°C, put the pre-sintered powders into a ball mill for wet ball milling, the speed of the ball mill is 30 rpm, the ball milling time is 34 hours, the ball milling media is distilled water and zirconia balls, and the mass ratio of zirconia balls: material to be ground: distilled water is 3:1:0.9. The mass ratio of large balls, medium balls, and small balls in zirconia balls is 1:2:3. Then dry, the drying temperature is 95°C, and the drying time is 17 hours. Put the dried mixed powder into a grinding jar for grinding for 30 minutes, sieve the ground mixed powder, the mesh number of the sieve is 180, and obtain (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 powder.
[0040] (2) Weigh SnO2 and PbO powders according to the chemical formula of PbSnO3. Pre-calculate SnO2 and PbO powders for 2 hours at a temperature of 840°C. Put the pre-calculated powders into a ball mill for wet milling. The speed of the ball mill is 28 rpm. The milling time is 38 hours. The milling media is distilled water and zirconia balls. The mass ratio of zirconia balls: milled material: distilled water is 3:1:0.9. The mass ratio of large balls, medium balls, and small balls in zirconia balls is 1:2:3. Then dry at a temperature of 95°C and a drying time of 18 hours. Put the dried mixed powder into a grinding jar for grinding for 30 minutes. Sieve the ground mixed powder with a mesh size of 180 to obtain PbSnO3 powder.
[0041] (3) The pre-sintered powder was heated to 0.03PbSnO 3- 0.97(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3Ti 1 / 3 )O3 chemical formula weigh PbSnO3 and (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3)O3 powder, put the mixed powder into a ball mill for wet ball milling, the speed of the ball mill is 33 rpm, the ball milling time is 38 hours, the ball milling medium is distilled water and zirconia balls, and the mass ratio of zirconia balls: material to be ground: distilled water is 3:1:0.9. The mass ratio of large balls, medium balls, and small balls in zirconia balls is 1:2:3. After that, the drying and drying temperature is 98°C, and the drying time is 15h. The dried mixed powder is put into a grinding jar for grinding for 31 minutes, and the ground mixed powder is sieved with a mesh size of 200 mesh. The sieved mixed medium entropy powder is pressed into tablets. The diameter of the mold used for tableting is 13mm, the uniaxial pressure is 175MPa, and the holding time is 11.5 minutes.
[0042] (4) The pressed unsintered ceramic sheet is placed in a muffle furnace and sintered at 1255°C in air. The same powder as the ceramic sheet is added around and on the top of the ceramic sheet for burial firing. The temperature of the muffle furnace is raised from room temperature to 1255°C at a heating rate of 4.5°C / min. The temperature is kept in the muffle furnace for 2.9 hours, and then the muffle furnace is cooled to a low temperature and taken out.
[0043] Figure 1 The xPbSnO prepared in Examples 1 to 3 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3Ti 1 / 3 )O3, (x = 0 ~ 0.03) composite phase entropy ceramics XRD spectrum; from Figure 1 It can be seen that the three medium-entropy ceramics all have a single-phase perovskite structure, and almost no impurities are visible.
[0044] Figure 2 The (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )SEM microstructure of O3 medium entropy ceramics. Figure 2 It can be seen that the relative density is high and the grains are irregular polygons.
[0045] Figure 3 The xPbSnO prepared in Examples 1 to 3 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf1 / 3 Zr 1 / 3Ti 1 / 3 )O3, (x = 0 ~ 0.03) composite phase medium entropy ceramic room temperature dielectric constant diagram; From the figure, it can be seen that at room temperature, under 1kHz frequency test, (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 dielectric constant is 825, much higher than the 100 of the base material. 0.015PbSnO 3- 0.985(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 composite medium entropy ceramic dielectric constant is 630, 0.03PbSnO 3- 0.97(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 composite medium entropy ceramic dielectric constant is 574. Compared with PbZrO3 matrix material, the dielectric constant is improved after A and B sites are doped with medium entropy and PbSnO3 is added.
[0046] Figure 4 The xPbSnO prepared in Examples 1 to 3 3- (1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3Ti 1 / 3 )O3, (x=0~0.03) composite phase medium entropy ceramic room temperature dielectric loss diagram; from Figure 4 It can be seen that at room temperature, under 1kHz frequency test, (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 dielectric loss is 0.043, 0.015PbSnO 3- 0.985(Pb 0.96 La 0.01Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 composite phase entropy ceramic dielectric loss is 0.027, 0.03PbSnO 3- 0.97(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 composite phase entropy ceramic dielectric loss is 0.006, 0.03PbSnO 3- 0.97(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 has the lowest dielectric loss at 1kHz.
Claims
1. A medium entropy lead zirconate based composite dielectric ceramic with dual doping at A and B sites, characterized in that: The medium entropy dielectric ceramic is designed for medium entropy at the B position and partially designed for medium entropy at the A position, and forms a composite ceramic with PbSnO3. The chemical formula of the medium entropy dielectric ceramic is: xPbSnO3–(1-x)(Pb 0.96 The 0.01 They 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 You 1 / 3 )O3,(x=0.0.03)。 2. The method for preparing the A and B-site dual-doped mid-entropy lead zirconate-based composite dielectric ceramic according to claim 1, characterized in that: The following steps are involved: (1) According to (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, weigh BaCO3, La2O3, Sm2O3, HfO2, ZrO2, TiO2 powders respectively, and weigh SnO2 and PbO powders respectively according to the chemical formula of PbSnO3; (2) The above powders were placed in a three-dimensional mixer for mixing for 30 to 50 minutes, and then pre-calcined. The pre-calcined powders were classified according to xPbSnO3–(1-x)(Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3 (x = 0 ~ 0.03) chemical formula weigh PbSnO3 and (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )O3, respectively put them into a ball mill for wet ball milling, and then grind, sieve and tablet press after drying; (3) The pressed unsintered ceramic pieces are placed in an alumina crucible, and the alumina crucible containing the ceramic pieces is placed in a muffle furnace for burial firing.
3. The method for preparing the A- and B-site dual-doped mid-entropy lead zirconate-based composite dielectric ceramic according to claim 2, characterized in that: The conditions for wet ball milling in step (2) are as follows: the rotation speed of the ball mill is 15 to 35 rpm, the ball milling time is 36 to 72 hours, the ball milling medium is distilled water and zirconia balls, the weight ratio of zirconia balls: material to be ground: distilled water is 3:0.9:1, and the mass ratio of large balls, medium balls, and small balls in the zirconia balls is 1:2:
3.
4. The method for preparing the A- and B-position dual-doped mid-entropy lead zirconate-based ceramic according to claim 2, characterized in that: The drying temperature in step (2) is 80 to 120° C. and the drying time is 12 to 20 hours.
5. The method for preparing the A- and B-site dual-doped mid-entropy lead zirconate-based composite dielectric ceramic according to claim 2, characterized in that: The grinding conditions in step (2) are as follows: the dried mixed powder is placed in a grinding jar and ground for 20 to 50 minutes, and the mesh size of the sieve is 80 to 200 meshes.
6. The method for preparing the A- and B-site dual-doped mid-entropy lead zirconate-based composite dielectric ceramic according to claim 2, characterized in that: The diameter of the mold used for tableting in step (2) is 10-13 mm, the uniaxial pressure is 160-180 MPa, and the holding time is 5-15 minutes.
7. The method for preparing the A- and B-site dual-doped mid-entropy lead zirconate-based composite dielectric ceramic according to claim 2, characterized in that: In step (2), (Pb 0.96 La 0.01 Ba 0.01 Sm 0.01 )(Hf 1 / 3 Zr 1 / 3 Ti 1 / 3 )The pre-sintering temperature of the O3 medium entropy ceramic powder is 800-850°C, and the holding time is 1.8-2.2h; the pre-sintering temperature of the PbSnO3 ceramic powder is 800-850°C, and the holding time is 1.7-2.3h.
8. The method for preparing the A- and B-site dual-doped mid-entropy lead zirconate-based composite dielectric ceramic according to claim 2, characterized in that: In step (3), the burying method is to add the same powder as the ceramic sheet around and on the top of the ceramic sheet for burying, and raise the temperature of the muffle furnace from room temperature to 1200-1270°C at a heating rate of 4.5°C / min. The insulation time in the muffle furnace is 2.8-3.2 hours, and then the furnace is cooled to a low temperature and taken out.
Citation Information
Patent Citations
A-site high-entropy perovskite oxide MeTiO3 thermoelectric ceramic and preparation method thereof
CN112960978A
Ceramic material for low-temperature co-fired ceramic capacitor and ceramic capacitor
CN113929459A
ABO3 type low dielectric loss ceramic and preparation method thereof
CN116924796A
A and B-site co-doped BaTiO3-based high-entropy dielectric film and preparation method thereof
CN117756171A
polycrystalline dielectric ceramic material dielectric devices