Refractory castable for A cover of main channel of blast furnace and preparation method of refractory castable
By using specific combinations of mullite particles and fine powders, as well as heat-resistant steel fibers, the refractory castable material of the A-cover of the blast furnace main groove is improved, and the problems of poor connection degree between aggregate and matrix and insufficient thermal shock stability are solved. Improves the strength and high temperature stability of the material and extends the service life.
Patent Information
- Application Number
- CN202410976861.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-21
- Publication Date
- 2024-11-08
AI Technical Summary
The refractory castable aggregate in the A-cover of the existing blast furnace main groove has poor connection with the matrix, which leads to easy peeling at high temperatures and insufficient thermal shock stability, affecting service life.
10-15 wt% mullite particles, 20-30 wt% 1-3 mm mullite particles, 10-15 wt% 0.1-1 mm mullite particles, 5-10 wt% sintered alumina particles, 10-20 wt. % mullite fine powder, 5-10 wt% alumina fine powder, 3-5 wt% silica fine powder, 5-10 wt% CA71 cement fine powder, 1-3 wt% aluminum powder, 3-5 wt% Silicon carbide fine powder and 1-2 wt% steel fibers improve the degree of connection between aggregate and matrix and thermal shock stability through specific mixing and baking processes.
It significantly improves the strength and high temperature stability of the refractory castable material, extends the service life of the A-cover of the blast furnace main groove, and generally increases by 1 times.
Smart Images

Figure BDA0004954841250000091 
Figure BDA0004954841250000101 
Figure BDA0004954841250000102
Abstract
Description
Technical Field
[0001] The invention relates to the field of refractory materials, and in particular to a refractory castable for a blast furnace main trench A cover and a preparation method thereof. Background Art
[0002] The blast furnace main trench A cover is a very important component in the blast furnace iron-making process. It is used to protect the blast furnace main trench and prevent impurities and heat from damaging the main trench during the smelting process. At the same time, it can also play a role in heat preservation to ensure the stability of the smelting process. The blast furnace main trench A calcium mainly prevents heat loss and reduces oxidation loss, so that the heat in the furnace can be more concentrated on the molten iron, reducing the temperature drop of the molten iron; at the same time, the main trench A cover can also effectively prevent slag and other impurities from entering the main trench, ensuring the purity and stability of the smelting process; in addition, it can also reduce the labor intensity of workers to a certain extent and improve the safety of the working environment.
[0003] At present, the A cover is mainly composed of steel structure, insulation layer and working layer. The insulation layer is mainly composed of porous insulating refractory castables, which have low thermal conductivity and good insulation effect. The working layer is composed of dense refractory castables, which are divided into two parts: aggregates of different grades and matrix with smaller particle size. The aggregates are sintered / electrofused dense aggregates with low surface roughness. The connection between the aggregates and the matrix is poor, and gaps often appear between the aggregates and the matrix. During use, due to the high temperature, the matrix shrinks, and the gap between the aggregates and the matrix becomes larger, which seriously causes the aggregates to peel off, resulting in a reduced lifespan. Secondly, during the iron-out and iron-out cycles, the working surface is subjected to huge thermal stress, which puts forward more stringent requirements on the thermal shock stability of the refractory castables of the working surface. The matrix is often more prone to cracks, resulting in partial peeling of the working surface. In addition, there is currently no patent for the A cover of the main trench of the blast furnace, so it is necessary to improve the existing dense refractory castables for the working surface and increase the service life of the A cover.
[0004] The present invention aims to overcome the defects of the prior art and provides a refractory castable for a long-life blast furnace main ditch A cover and a preparation method thereof. The prepared refractory castable for a long-life blast furnace main ditch A cover has good aggregate connection with the matrix, high strength, excellent high-temperature stability, excellent thermal shock stability, and the service life is generally increased by 1 times. Summary of the invention
[0005] The object of the present invention is to provide a refractory castable for a blast furnace main trench A cover and a preparation method thereof in view of the above problems.
[0006] The object of the present invention is achieved in this way: a refractory castable for a blast furnace main trench A cover, the refractory castable body consisting of 10-15wt% of 3-5mm mullite particles, 20-30wt% of 1-3mm mullite particles, 10-15wt% of 0.1-1mm mullite particles, 5-10wt% of 1-3mm sintered alumina particles, 10-20wt% of mullite fine powder, 5-10wt% of alumina micropowder, 3-5wt% of silicon dioxide micropowder, 5-10wt% of CA71 cement fine powder, 1-3wt% of aluminum powder, 3-5wt% of silicon carbide fine powder and 1-2wt% of steel fiber.
[0007] A preparation method of a refractory castable for a blast furnace main trench A cover comprises the following steps: step 1: adding 10-20wt% of mullite fine powder, 5-10wt% of alumina micropowder, 3-5wt% of silicon dioxide micropowder and 5-10wt% of CA71 cement fine powder into a mixer and mixing for 2-4h, and obtaining a premixed fine powder after uniform mixing; step 2: pouring 10-15wt% of 3-5mm mullite particles, 20-30wt% of 1-3mm mullite particles, 10-15wt% of 0.1-1mm mullite particles and 5-10wt% of 1-3mm sintered alumina particles into a mixer and stirring for 5-10min, adding 1-3wt% of aluminum powder and 3-5wt% of silicon carbide fine powder while stirring, and adding 0.1-0.5mg / m 2 1-2wt% water of the water reducer, then add the premixed fine powder and stir for 5-10min, add 1-2wt% of steel fiber while stirring, and add 2-4wt% of water after the particles and fine powder are evenly mixed, and then mix evenly to obtain a refractory castable; Step three: Pour the refractory castable into the steel structure on which the insulation layer has been poured. The pouring process must not be interrupted. After pouring, cure at room temperature for 36-60h, and then bake at 80-100℃ for 48-72h, 150-200℃ for 48-72h, and 250-300℃ for 36-48h to obtain a complete blast furnace main trench A cover.
[0008] The particle size of the mullite fine powder described in step one is less than or equal to 0.088mm, the Al2O3 content is greater than or equal to 65wt%, the pore size is bimodal distribution, the pores less than 1μm account for not less than 50vol%, and the median pore size is less than 1μm; the Al2O3 content of the alumina micropowder is greater than or equal to 93wt%, and the particle size is less than or equal to 44μm; the SiO2 content of the silica micropowder is greater than or equal to 92%, and the particle size is less than or equal to 44μm; the Al2O3 content of the CA71 cement fine powder is greater than or equal to 68wt%, K2O+Na2O is less than or equal to 0.4wt%, the particle size is less than or equal to 88μm, and the refractoriness is 1580-2000℃.
[0009] The Al2O3 content of all the mullite particles in step 2 is greater than or equal to 65wt%, the pore size is bimodal, the pore size less than 1μm accounts for no less than 50vol%, the median pore size is less than 1μm, and the volume density is 1.66-2.01g / cm 3 The apparent porosity is 21.2-38.4%, the closed porosity is 9.8-17.5%; the Al2O3 content of the sintered alumina particles is 68-75%, and the volume density is 3.45-3.60g / cm 3 , the apparent porosity is below 5.0%; the aluminum powder Al content is greater than or equal to 99.5wt%, the particle size is less than or equal to 74μm, and the median particle size is less than 35μm; the silicon carbide fine powder SiC content is greater than or equal to 97wt%, and the particle size is less than or equal to 88μm; the steel fiber Cr content is 23-27wt%, the melting temperature is 1425-1510℃, the critical oxidation temperature under continuous use conditions is 1100-1200℃, and the tensile strength at 870℃ is 50-200MPa; the water reducer is a mixture of naphthalenesulfonate formaldehyde condensate and melamine sulfonate formaldehyde condensate, with a ratio of 1:1.
[0010] The beneficial effects of the present invention are as follows: the mullite particles and fine powder used in the present invention are mainly mullite phase, the pore size is bimodal distribution, and the pores less than 1 μm account for no less than 50 vol%, the median pore size is less than 1 μm, the porosity is relatively high, and therefore the surface roughness is relatively large; using it as a raw material, or increasing the contact area with the surrounding materials, forming meshing, reducing or even eliminating the gap between the aggregate and the matrix, while increasing the thermal shock stability and strength of the refractory castable, and improving the stability of the material at high temperatures. At the same time, due to the small pore size and large porosity, using it as an aggregate can significantly reduce the thermal conductivity and increase the insulation effect of the blast furnace main trench A cover. Compared with the existing dense castable, the difference in properties between the working layer and the insulation layer is too large, and after using the mullite particles and fine powder, the difference can be reduced, and the insulation layer and the working layer can have better compatibility, and it is not easy to peel off between the two layers.
[0011] In order to further improve the toughness of the refractory castable used for the working surface of the main trench A cover of the blast furnace, reduce spalling, and improve thermal shock stability, heat-resistant steel fibers are added to the refractory castable. The strong drawing power of the heat-resistant steel fiber will effectively prevent the propagation of cracks caused by thermal stress; its good antioxidant ability enables it to be effective from the beginning to the end of service, and at the same time reduce or even eliminate cracking caused by temperature changes during the curing and baking process of the refractory castable.
[0012] The addition of SiC fine powder and aluminum powder plays the role of explosion-proof agent, preventing the cracking of the A-cap finished product; on the other hand, at high temperatures, SiC or mullite whiskers will be formed at places where the interface energy between the aggregate and the matrix is large, further increasing the high-temperature volume stability while improving the high-temperature flexural strength and reducing thermal spalling. In addition, SiC whiskers are also a good sunscreen, which will further reduce the heat loss caused by thermal radiation.
[0013] The use of high-efficiency composite water reducing agent can reduce the water content of refractory castables to about 5wt%. The reduction of water content not only reduces the porosity, eliminates cracking during the curing and baking stages, reduces the number of cracks, and improves the strength; it can also improve the high-temperature volume stability of refractory castables, reduce high-temperature thermal stress and reduce the source of crack expansion, and improve thermal shock stability.
[0014] Baking temperature 80-100℃: Loss of free water, heat and moisture transfer are best in this temperature range. 150-200℃: Water vapor is generated, dehydration. 250-300℃: Dehydration of hydration products.
[0015] The refractory castable for the long-life blast furnace main trench A cover prepared by the present invention is tested to have an apparent porosity of 25.4-40.1% and a bulk density of 1.96-2.31 / cm 3 ; Compressive strength 60.0-125MPa; flexural strength 10-25MPa, compressive strength retention rate after one thermal shock at 1100℃ is 50.2-97.4%, flexural strength retention rate is 29.2-72.6%, and the line change at 1550℃ is -0.12-0.09%.
[0016] Therefore, the refractory castable for the long-life blast furnace main ditch A cover prepared by the present invention and the preparation method thereof have good aggregate connection with the matrix, high strength, excellent high-temperature stability, excellent thermal shock stability, and the service life is generally increased by 1 times. DETAILED DESCRIPTION
[0017] The technical solution adopted by the present invention is: a refractory castable for a long-life blast furnace main trench A cover and a preparation method thereof, wherein the steps of the preparation method are: step 1: adding 10-20wt% of mullite fine powder, 5-10wt% of alumina micropowder, 3-5wt% of silica micropowder, and 5-10wt% of CA71 cement fine powder into a mixer and mixing for 2-4h, and obtaining a premixed fine powder after mixing evenly.
[0018] Step 2: Pour 10-15wt% of 3-5mm mullite particles, 20-30wt% of 1-3mm mullite particles, 10-15wt% of 0.1-1mm mullite particles, and 5-10wt% of 1-3mm sintered alumina particles into a mixer and stir for 5-10 minutes, add 1-3wt% of aluminum powder and 3-5wt% of silicon carbide fine powder while stirring, and after mixing evenly, add 0.1-0.5mg / m 2 1-2wt% water of the water reducer. Then add the premixed fine powder and stir for 5-10 minutes, add 1-2wt% steel fiber while stirring, add 2-4wt% water after the particles and fine powder are evenly mixed, and then mix evenly to obtain a refractory castable.
[0019] Step 3: Pour the refractory castable into the completed steel structure on which the insulation layer has been poured. The pouring process must not be interrupted. After pouring, cure it at room temperature for 36-60 hours, then bake it at 80-100℃ for 48-72 hours, 150-200℃ for 48-72 hours, and 250-300℃ for 36-48 hours to obtain a complete blast furnace main trench A cover.
[0020] The particle size of the mullite fine powder is less than or equal to 0.088 mm, the Al2O3 content is greater than or equal to 65wt%, the pore diameter is bimodal distribution, the pores less than 1μm account for not less than 50vol%, and the median pore diameter is less than 1μm.
[0021] The aluminum oxide powder has an Al2O3 content greater than or equal to 93wt% and a particle size less than or equal to 44μm.
[0022] The SiO2 content of the silicon dioxide powder is greater than or equal to 92%, and the particle size is less than or equal to 44 μm.
[0023] The CA71 cement fine powder has an Al2O3 content greater than or equal to 68wt%, a K2O+Na2O content less than or equal to 0.4wt%, a particle size less than or equal to 88μm, and a refractoriness of 1580-2000°C.
[0024] The mullite particles (0.1-1 mm, 1-3 mm, 3-5 mm) have an Al2O3 content greater than or equal to 65 wt%, a bimodal distribution of pore diameters, a pore size less than 1 μm accounting for no less than 50 vol%, a median pore size less than 1 μm, and a volume density of 1.66-2.01 g / cm 3 The apparent porosity is 21.2-38.4%, and the closed porosity is 9.8-17.5%.
[0025] The sintered alumina particles have an Al2O3 content of 68-75% and a bulk density of 3.45-3.60 g / cm 3 , the apparent porosity is below 5.0%.
[0026] The aluminum powder has an Al content greater than or equal to 99.5wt%, a particle size less than or equal to 74μm, and a median particle size less than 35μm.
[0027] The silicon carbide fine powder has a SiC content greater than or equal to 97wt% and a particle size less than or equal to 88μm.
[0028] The steel fiber has a Cr content of 23-27 wt %, a melting temperature of 1425-1510° C., a critical oxidation temperature of 1100-1200° C. under continuous use conditions, and a tensile strength of 50-200 MPa at 870° C.
[0029] The water reducing agent is a mixture of naphthalene sulfonate formaldehyde condensate and melamine sulfonate formaldehyde condensate in a ratio of 1:1.
[0030] The rotating speed of the mixer can reach 1500r / min, and the model is EIRICH DW31 / 7 powerful mixer.
[0031] The mixer is a planetary mixer, model EIRICH RV24.
[0032] The present invention is further described below in conjunction with specific implementation modes, but is not intended to limit the protection scope thereof.
[0033] To avoid repetition, the equipment and materials involved in the specific implementation method are described as follows and will not be repeated in the examples: the particle size of the mullite fine powder is less than or equal to 0.088 mm, the Al2O3 content is greater than or equal to 65wt%, the pore size is bimodal distribution, the proportion of pores less than 1μm is not less than 50vol%, and the median pore size is less than 1μm.
[0034] The aluminum oxide powder has an Al2O3 content greater than or equal to 93wt% and a particle size less than or equal to 44μm.
[0035] The SiO2 content of the silicon dioxide powder is greater than or equal to 92%, and the particle size is less than or equal to 44 μm.
[0036] The CA71 cement fine powder has an Al2O3 content greater than or equal to 93wt%, a K2O+Na2O content less than or equal to 0.4wt%, a particle size less than or equal to 88μm, and a refractoriness greater than or equal to 1580°C.
[0037] The mullite temperature is 1425, the Al2O3 content of the stone particles (0.1-1mm, 1-3mm, 3-5mm) is greater than or equal to 65wt%, the pore size is bimodal, the pores less than 1μm account for no less than 50vol%, the median pore size is less than 1μm, and the volume density is 1.66-2.01g / cm 3The apparent porosity is 21.2-38.4%, and the closed porosity is 9.8-17.5%.
[0038] The sintered alumina particles have an Al2O3 content of 68-75% and a bulk density of 3.45-3.60 g / cm 3 , the apparent porosity is below 5.0%.
[0039] The aluminum powder has an Al content greater than or equal to 99.5wt%, a particle size less than or equal to 74μm, and a median particle size less than 35μm.
[0040] The silicon carbide fine powder has a SiC content greater than or equal to 97wt% and a particle size less than or equal to 88μm.
[0041] The steel fiber has a Cr content of 23-27 wt %, a melting temperature of 1425-1510° C., a critical oxidation temperature of 1100-1200° C. under continuous use conditions, and a tensile strength of 50-200 MPa at 870° C.
[0042] The water reducing agent is a mixture of naphthalene sulfonate formaldehyde condensate and melamine sulfonate formaldehyde condensate in a ratio of 1:1.
[0043] The rotating speed of the mixer can reach 1500r / min, and the model is EIRICH DW31 / 7 powerful mixer.
[0044] The mixer is a planetary mixer, model EIRICH RV24.
[0045] Example 1
[0046] A refractory castable for a long-life blast furnace main trench A cover and a preparation method thereof. The steps of the preparation method described in this embodiment are: Step 1: 17wt% of mullite fine powder, 7wt% of alumina fine powder, 3wt% of silica fine powder, and 7wt% of CA71 cement fine powder are added to a mixer and mixed for 2h to obtain a premixed fine powder after uniform mixing.
[0047] Step 2: Pour 15wt% of 3-5mm mullite particles, 30wt% of 1-3mm mullite particles, 10wt% of 0.1-1mm mullite particles, and 5wt% of 1-3mm sintered alumina particles into a mixer and stir for 8 minutes. Add 2wt% of aluminum powder and 4wt% of silicon carbide fine powder while stirring. After mixing evenly, add 0.5mg / m 2 1wt% water of water reducing agent. Then add premixed fine powder and stir for 10 minutes, add 2wt% steel fiber while stirring, add 4wt% water after the particles and fine powder are evenly mixed, and obtain refractory castable after evenly mixing.
[0048] Step 3: Pour the refractory castable into the completed steel structure with the insulation layer poured. The pouring process must not be interrupted. After pouring, cure it at room temperature for 48 hours, then bake it at 80-100℃ for 48 hours, 150-200℃ for 48 hours, and 250-300℃ for 36 hours to obtain a complete blast furnace main trench A cover.
[0049] This embodiment uses four kinds of mullite particles (aggregates), and the aggregates used are existing dense aggregate, mullite aggregate 1, mullite aggregate 2, and mullite aggregate 3, respectively, and their properties are shown in the following table.
[0050]
[0051]
[0052] The properties of the refractory castable (mullite aggregates 1, 2, and 3) for the long-life blast furnace main trench A cover prepared in this embodiment are shown in the following table.
[0053]
[0054] Example 2
[0055] A refractory castable for a long-life blast furnace main trench A cover and a preparation method thereof. The preparation method described in this embodiment comprises the following steps: Step 1: 20 wt% of mullite fine powder, 10 wt% of alumina fine powder, 4 wt% of silica fine powder, and 10 wt% of CA71 cement fine powder are added to a mixer and mixed for 3 hours to obtain a premixed fine powder after uniform mixing.
[0056] Step 2: Pour 10wt% of 3-5mm mullite particles, 20wt% of 1-3mm mullite particles, 12wt% of 0.1-1mm mullite particles, and 8wt% of 1-3mm sintered alumina particles into a mixer and stir for 5 minutes. Add 1wt% of aluminum powder and 5wt% of silicon carbide fine powder while stirring. After mixing evenly, add 0.1mg / m 2 2wt% water of water reducing agent. Then add premixed fine powder and stir for 5 minutes, add 1wt% steel fiber while stirring, add 2wt% water after the particles and fine powder are evenly mixed, and mix evenly to obtain refractory castable.
[0057] Step 3: Pour the refractory castable into the completed steel structure with the insulation layer poured. The pouring process must not be interrupted. After pouring, cure it at room temperature for 36 hours, then bake it at 80-100℃ for 60 hours, 150-200℃ for 60 hours, and 250-300℃ for 48 hours to obtain a complete blast furnace main trench A cover.
[0058] This embodiment uses four kinds of mullite particles (aggregates), and the aggregates used are existing dense aggregate, mullite aggregate 1, mullite aggregate 2, and mullite aggregate 3, respectively, and their properties are shown in the following table.
[0059]
[0060] The properties of the refractory castable (mullite aggregates 1, 2, and 3) for the long-life blast furnace main trench A cover prepared in this embodiment are shown in the following table.
[0061]
[0062]
[0063] Example 3
[0064] A refractory castable for a long-life blast furnace main trench A cover and a preparation method thereof. The preparation method described in this embodiment comprises the following steps: Step 1: 10 wt% of mullite fine powder, 5 wt% of alumina fine powder, 5 wt% of silica fine powder, and 5 wt% of CA71 cement fine powder are added to a mixer and mixed for 4 hours to obtain a premixed fine powder after uniform mixing.
[0065] Step 2: Pour 14wt% of 3-5mm mullite particles, 30wt% of 1-3mm mullite particles, 15wt% of 0.1-1mm mullite particles, and 10wt% of 1-3mm sintered alumina particles into a mixer and stir for 10 minutes, add 3wt% of aluminum powder and 3wt% of silicon carbide fine powder while stirring, and after mixing evenly, add 0.3mg / m 2 1.5wt% water of water reducing agent. Then add premixed fine powder and stir for 10 minutes, add 2wt% steel fiber while stirring, add 4wt% water after the particles and fine powder are evenly mixed, and mix well to obtain refractory castable.
[0066] Step 3: Pour the refractory castable into the completed steel structure with the insulation layer poured. The pouring process must not be interrupted. After pouring, cure it at room temperature for 60 hours, then bake it at 80-100℃ for 72 hours, 150-200℃ for 72 hours, and 250-300℃ for 48 hours to obtain a complete blast furnace main trench A cover.
[0067] This embodiment uses four kinds of mullite particles (aggregates), and the aggregates used are existing dense aggregate, mullite aggregate 1, mullite aggregate 2, and mullite aggregate 3, respectively, and their properties are shown in the following table.
[0068]
[0069]
[0070] The properties of the refractory castable (mullite aggregates 1, 2, and 3) for the long-life blast furnace main trench A cover prepared in this embodiment are shown in the following table.
[0071]
[0072] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.
Claims
1. A refractory castable for a blast furnace main trench A cover, characterized in that: The refractory castable body consists of 10-15wt% of 3-5mm mullite particles, 20-30wt% of 1-3mm mullite particles, 10-15wt% of 0.1-1mm mullite particles, 5-10wt% of 1-3mm sintered alumina particles, 10-20wt% of mullite fine powder, 5-10wt% of alumina micropowder, 3-5wt% of silicon dioxide micropowder, 5-10wt% of CA71 cement fine powder, 1-3wt% of aluminum powder, 3-5wt% of silicon carbide fine powder and 1-2wt% of steel fiber.
2. A method for preparing a refractory castable for a blast furnace main trench A cover, characterized in that: The following steps are involved: Step 1: Add 10-20wt% of mullite fine powder, 5-10wt% of alumina fine powder, 3-5wt% of silica fine powder, and 5-10wt% of CA71 cement fine powder into a mixer and mix for 2-4h to obtain premixed fine powder after mixing evenly; Step 2: Pour 10-15wt% of 3-5mm mullite particles, 20-30wt% of 1-3mm mullite particles, 10-15wt% of 0.1-1mm mullite particles, and 5-10wt% of 1-3mm sintered alumina particles into a mixer and stir for 5-10 minutes. Add 1-3wt% of aluminum powder and 3-5wt% of silicon carbide fine powder while stirring. After mixing evenly, add 0.1-0.5mg / m 2 1-2wt% water of water reducer, then add premixed fine powder and stir for 5-10min, add 1-2wt% steel fiber while stirring, add 2-4wt% water after the particles and fine powder are evenly mixed, and then mix well to obtain refractory castable; Step 3: Pour the refractory castable into the steel structure on which the insulation layer has been poured. The pouring process must not be interrupted. After pouring, cure it at room temperature for 36-60 hours, then bake it at 80-100℃ for 48-72 hours, 150-200℃ for 48-72 hours, and 250-300℃ for 36-48 hours to obtain a complete blast furnace main trench A cover.
3. The method for preparing a refractory castable for a blast furnace main trench A cover according to claim 2, characterized in that: The particle size of the mullite fine powder in step one is less than or equal to 0.088mm, the Al2O3 content is greater than or equal to 65wt%, the pore size is bimodal distribution, the pore size less than 1μm accounts for not less than 50vol%, and the median pore size is less than 1μm; the Al2O3 content of the alumina powder is greater than or equal to 93wt%, and the particle size is less than or equal to 44μm; the SiO2 content of the silica powder is greater than or equal to 92%, and the particle size is less than or equal to 44μm; the Al2O3 content of the CA71 cement fine powder is greater than or equal to 68wt%, K2O+Na2O is less than or equal to 0.4wt%, the particle size is less than or equal to 88μm, and the refractoriness is 1580-2000℃.
4. The method for preparing a refractory castable for a blast furnace main trench A cover according to claim 2, characterized in that: The Al2O3 content of all the mullite particles in step 2 is greater than or equal to 65wt%, the pore size is bimodal, the pore size less than 1μm accounts for no less than 50vol%, the median pore size is less than 1μm, and the volume density is 1.66-2.01g / cm 3 The apparent porosity is 21.2-38.4%, the closed porosity is 9.8-17.5%; the Al2O3 content of the sintered alumina particles is 68-75%, and the bulk density is 3.45-3.60 g / cm 3 , the apparent porosity is below 5.0%; the Al content of the aluminum powder is greater than or equal to 99.5wt%, the particle size is less than or equal to 74μm, and the median particle size is less than 35μm; the SiC content of the silicon carbide fine powder is greater than or equal to 97wt%, and the particle size is less than or equal to 88μm; the Cr content of the steel fiber is 23-27wt%, the melting temperature is 1425-1510℃, the critical oxidation temperature under continuous use conditions is 1100-1200℃, and the tensile strength at 870℃ is 50-200MPa; the water reducer is a mixture of naphthalenesulfonate formaldehyde condensate and melamine sulfonate formaldehyde condensate, with a ratio of 1:1.
Citation Information
Patent Citations
High-strength mullite pouring material for cement kiln
CN102491767A
Refractory castable for repairing of blast furnace iron mouth
CN108503373A
Castable for permanent layer of continuous casting tundish
CN110467472A
Mullite refractory castable for ultrahigh-temperature smelting
CN111704474A
Lightweight high-strength mullite castable and construction method
CN114230350A