Device and method for reinforcing rock cultural relics
The dense aluminum phosphate protective layer was formed on carbonate rocky cultural relics through electrochemical deposition, which solved the problems of coating cracking and insufficient acid resistance, and significantly improved the weather resistance and acid resistance of cultural relics.
Patent Information
- Application Number
- CN202410974983.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing aluminum phosphate reinforcement methods often cause coating cracking problems on carbonate rock cultural relics, resulting in poor acid resistance and inability to effectively prevent dissolution and cracking.
The electrochemical deposition method is used to form an aluminum phosphate precipitation protective layer on the surface and inside of the weathered carbonate rock. By precipitation of aluminum ions and phosphate ions under the external electric field, a dense protective layer is formed to avoid cracking and improve acid resistance.
The protective layer formed is dense and has low porosity, effectively avoids cracking, and significantly improves the acid resistance of the aluminum phosphate protective layer, ensuring the artistic and historical value of the cultural relics.
Smart Images

Figure CN118908748A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cultural relics protection, and in particular to a device and method for reinforcing rock cultural relics. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Among rock cultural relics, carbonate rock cultural relics are extremely susceptible to corrosion and other diseases caused by water and acid in the preservation environment, resulting in cracking, discoloration and other problems, which seriously affect the historical and artistic value of carbonate rock cultural relics. In order to prevent carbonate rock cultural relics from being corroded, materials such as calcium oxalate, hydroxyapatite or aluminum phosphate are often used for reinforcement. However, studies have found that calcium oxalate materials have low permeability due to their rapid reaction with calcium carbonate, and the thickness of the reinforcement layer formed is thin, which cannot completely avoid problems such as falling off and cracking; hydroxyapatite materials have a moderate reaction time with calcium carbonate, but there is a lattice mismatch problem between it and calcium carbonate crystals, which leads to the acid resistance of the coating not meeting expectations; aluminum phosphate materials have a more similar crystal form to calcium carbonate, and the acid resistance of aluminum phosphate is much higher than that of calcium carbonate, so it can play a good reinforcement and protection effect.
[0004] The current aluminum phosphate reinforcement method commonly used is the dripping method or the capillary water absorption method, which is to add a liquid containing aluminum phosphate reinforcement material to the weathered carbonate rock, so that the aluminum phosphate component is affected by gravity or capillary force and penetrates into the cracks of the carbonate rock to achieve the purpose of reinforcement and protection. However, this method currently used still has the problem of coating cracking, resulting in limited improvement in acid resistance. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a device and method for reinforcing rock cultural relics, which uses electrochemical deposition to produce aluminum phosphate precipitation on the surface and inside of weathered carbonate rock to form an aluminum phosphate protective coating, thereby effectively avoiding cracking of the protective layer and improving acid resistance.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] A first aspect of the present invention provides a device for reinforcing rock cultural relics, comprising:
[0008] An electrochemical deposition cell, wherein one end of the electrochemical deposition cell is provided with an electrode connected to the positive electrode of a power source, and the other end thereof is provided with an electrode connected to the negative electrode of the power source;
[0009] The two end electrodes in the electrochemical deposition cell are provided with a first buffer sponge, a first agar spacer, an AlCl 3 Pasting materials, weathered stone storage room, (NH 4 ) 2 HPO 4 patch material, a second agar septum, and a second buffer sponge;
[0010] The first buffer sponge and the second buffer sponge are soaked with phosphate buffer;
[0011] The AlCl 3 The raw materials for preparing the patch material include cellulose and AlCl with a concentration of 0.1 to 0.2 M. 3 Aqueous solution, cellulose and AlCl 3 The mass ratio of the aqueous solution is 1:2-3;
[0012] The (NH 4 ) 2 HPO 4 The raw materials for preparing the patch material include cellulose and (NH 4 ) 2 HPO 4 Aqueous solution, cellulose and (NH 4 ) 2 HPO 4 The mass ratio of the aqueous solution is 1:2-3;
[0013] The outer wall of the weathered stone placement chamber is made of porous material and is used for placing rock cultural relics to be reinforced.
[0014] Optionally, the sponges in the first buffer sponge and the second buffer sponge are nano sponges.
[0015] Optionally, the phosphate buffer has a neutral pH value and includes potassium dihydrogen phosphate, sodium hydroxide and water.
[0016] Optionally, in the phosphate buffer, the concentration of potassium dihydrogen phosphate is 0.04-0.06M.
[0017] Optionally, the raw materials for preparing the first agar spacer and the second agar spacer include agar and water in a mass ratio of (4-8):96.
[0018] Optionally, the porous material of the weathered stone placement room includes one or more of gauze, non-woven fabric and rice paper.
[0019] Optionally, the rock cultural relics to be reinforced are made of carbonate rock.
[0020] Optionally, the electrodes in the electrochemical deposition cell are connected to the power supply via wires.
[0021] In a second aspect, a method for reinforcing rock cultural relics using the above-mentioned device for reinforcing rock cultural relics comprises the steps of:
[0022] S1. Wrap the rock cultural relics to be reinforced with porous materials, and immerse the porous materials in neutral phosphate buffer to obtain a weathered stone placement chamber;
[0023] S2. Connect one side of the weathered stone placement room to A l C l 3 The patch material, the first agar septum and the first buffer sponge are connected in sequence on the other side of the Fenghua material placement chamber (NH 4 ) 2 HPO 4 patch material, a second agar septum, and a second buffer sponge;
[0024] S3. Connect the first buffer sponge to the positive pole of the power supply, connect the second buffer sponge to the negative pole of the power supply, start the power supply and maintain the set time to complete the reinforcement of the rock cultural relics.
[0025] Optionally, start the power supply and set it to: current 30±5mA, voltage 120±10V, power-on time 24±4h.
[0026] The beneficial effects of the present invention are as follows:
[0027] 1. The device and method of the present invention can produce aluminum phosphate precipitation on the surface and inside of weathered carbonate rock by electrochemical deposition, and aluminum ions and phosphate ions form a precipitation protective layer under the action of an external electric field. The obtained protective layer is dense and has low porosity, which can effectively avoid cracking and improve the acid resistance of the aluminum phosphate protective layer.
[0028] 2. The present invention sets up a weathered stone placement chamber of porous material to avoid direct contact between the stone and the pasting material, prevent the reactants from gathering in a small range, and effectively improve the uniformity and density of the protective layer.
[0029] 3. The protective layer prepared by the present invention has moderate thickness, good color protection ability, and the color change of the sample is not obvious, which can effectively protect the artistic value of the cultural relics. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0031] In order to show the positions of various parts, the distances or sizes between them are exaggerated in the figure, and the schematic diagram is for illustration only.
[0032] Figure 1 It is a schematic diagram of the structure of the device for reinforcing rock cultural relics in Example 1.
[0033] Among them, 1. simulated weathering sample; 2. gauze; 3. Al Cl 3 Application material; 4. (NH 4 ) 2 HPO 4 Application material; 5. first agar spacer; 6. second agar spacer; 7. first buffer sponge; 8. second buffer sponge; 10. electrode material; 11. power supply. DETAILED DESCRIPTION
[0034] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0035] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0036] A device for reinforcing rock cultural relics, comprising:
[0037] An electrochemical deposition cell, wherein one end of the electrochemical deposition cell is provided with an electrode connected to the positive pole of a power source, and the other end of the electrochemical deposition cell is provided with an electrode connected to the negative pole of the power source;
[0038] The first buffer sponge, the first agar spacer, the AlCl 3 Pasting materials, weathered stone storage room, (NH 4 ) 2 HPO 4 patch material, a second agar septum, and a second buffer sponge;
[0039] The first buffer sponge and the second buffer sponge are soaked with phosphate buffer;
[0040] AlCl 3 The raw materials for preparing the patch material include cellulose and AlCl with a concentration of 0.1 to 0.2 M. 3 Aqueous solution, cellulose and AlCl 3The mass ratio of the aqueous solution is 1:2-3;
[0041] (NH 4 ) 2 HPO 4 The raw materials for preparing the patch material include cellulose and (NH 4 ) 2 HPO 4 Aqueous solution, cellulose and (NH 4 ) 2 HPO 4 The mass ratio of the aqueous solution is 1:2-3;
[0042] The outer wall of the weathered stone storage room is made of porous material and is used to place rock artifacts to be reinforced.
[0043] Through the above settings, aluminum phosphate precipitation is produced on the surface and inside of weathered carbonate rocks by electrochemical deposition. Aluminum ions and phosphate ions gradually diffuse into the porous material of the weathered stone placement room under the action of an external electric field, and diffuse into the surface and cracks of the rock cultural relics inside, and form a precipitation protective layer at this location. The obtained protective layer is dense and has low porosity, which can effectively avoid cracking, thereby preventing acid from penetrating into the cracks and improving acid resistance.
[0044] Optionally, the sponges in the first buffer sponge and the second buffer sponge are nano sponges, which play the role of fixing the buffer.
[0045] Optionally, the pH value of the phosphate buffer is neutral, and it includes potassium dihydrogen phosphate, sodium hydroxide and water; the sodium hydroxide serves as a pH adjuster.
[0046] Optionally, the concentration of potassium dihydrogen phosphate is 0.04-0.06M, which serves to neutralize the acid generated by electrolyzed water.
[0047] Optionally, the raw materials for preparing the first agar spacer and the second agar spacer include agar and water in a mass ratio of (4-8):96; the agar gel acts as a barrier, provides conductivity and electrolyzes water, and can also reduce precipitation formed by phosphate buffer and aluminum chloride.
[0048] Optionally, the porous material of the weathered stone placement room includes: one or more of gauze, non-woven fabric and rice paper; avoiding direct contact between the stone and the pasting material is conducive to the uniform diffusion of ions in the pasting material.
[0049] Optionally, the rock cultural relics to be reinforced are made of carbonate rock, specifically calcium carbonate rock material, which is more similar to aluminum phosphate in crystal form and can achieve better reinforcement and protection effect.
[0050] Optionally, the electrodes in the electrochemical deposition cell are connected to the power supply via wires to avoid forming a conductive loop outside the set conductive path, thereby preventing the generation effect of the protective layer from being reduced.
[0051] A method for reinforcing rock cultural relics using the above-mentioned device for reinforcing rock cultural relics comprises the steps of:
[0052] S1. Use porous materials to wrap the rock cultural relics to be reinforced to obtain a weathered stone storage room;
[0053] S2. Connect one side of the weathered stone placement room to A l C l 3 The patch material, the first agar septum and the first buffer sponge are connected in sequence on the other side of the Fenghua material placement chamber (NH 4 ) 2 HPO 4 patch material, a second agar septum, and a second buffer sponge;
[0054] S3. Connect the first buffer sponge to the positive pole of the power supply, connect the second buffer sponge to the negative pole of the power supply, start the power supply and maintain the set time to complete the reinforcement of the rock cultural relics.
[0055] Through the above process, a relatively dense and uniform aluminum phosphate protective layer can be formed on the cultural relics, effectively improving the cultural relics' resistance to weathering and acid.
[0056] Optionally, the power supply is set to: current 30±5mA, voltage 120±10V; power-on time is 24±4h; it needs to be adjusted according to the thickness of the protective layer to be generated and the size of the surface area of the cultural relic.
[0057] Example 1
[0058] Preparation of AlCl 3 Patching materials: First, add 1.33 g of aluminum chloride to 100 ml of deionized water to prepare a 0.1 M AlCl solution. 3 Aqueous solution, AlCl 3 The aqueous solution and cellulose were mixed in a ratio of 2:1 (w:w) to obtain a gel-like AlCl 3 Application material.
[0059] Preparation of (NH 4 ) 2 HPO 4 Patch material: First, add 1.32g diammonium hydrogen phosphate into 100ml deionized water to prepare a concentration of 0.1M (NH 4 ) 2 HPO 4 Aqueous solution, to prepare the obtained (NH 4 )2 HPO 4 Aqueous solution: cellulose = 2:1 (w:w) ratio mixed evenly to obtain a gel (NH 4 ) 2 HPO 4 Application material.
[0060] Preparation of agar septa: 4 g of agar powder was placed in a beaker, 96 g of deionized water was added, and the mixture was heated in a water bath (the temperature of the water bath was set to 92°C), and the mixture was stirred and mixed evenly. After about 30 minutes, the mixture was taken out of the water bath, poured into a plastic square box and cooled to room temperature to obtain a nearly transparent gel solid, i.e., the agar septa. The agar material was derived from HEOWNS and had a biological grade purity. The agar material was divided into a first agar pad and a second agar septum.
[0061] Preparation of phosphate buffer: Take 0.68 g of potassium dihydrogen phosphate, add 29.1 ml of 0.1 mol / L sodium hydroxide solution, and dilute with water to 100 ml. Both potassium dihydrogen phosphate and sodium hydroxide are produced by Sinopharm Group with analytical purity and have not been purified.
[0062] like Figure 1 As shown in the figure, the simulated weathering sample 1 (calcium carbonate stone) is wrapped with gauze 2 to form a weathered stone placement room to prevent the simulated weathering sample 1 from directly contacting the pasting material; AlCl is pasted on the anode of the weathered stone placement room. 3 Paste material 3, paste on the cathode side of the weathered stone storage room (NH 4 ) 2 HPO 4 A patch material 4 is provided, and a first agar spacer 5 and a second agar spacer 6 are respectively arranged on the outside of the two patch materials. Nanosponges with 5 ml of phosphate buffer are placed on the outside of the two agar spacers, respectively, as the first buffer sponge 7 and the second buffer sponge 8, which play a role in neutralizing the acid produced by electrolyzed water. The first buffer sponge 7 and the second buffer sponge 8 are respectively connected to the electrode material 10, and the electrode material 10 is respectively connected to the power supply 11, so as to obtain a device for reinforcing rock cultural relics on which the rock cultural relics to be reinforced are placed.
[0063] In this embodiment, the electrode material 10 is graphite. Along the current conduction direction, that is, from left to right in the figure, the thickness of the first buffer sponge 7 is 10 mm, the thickness of the first agar spacer 5 is 5 mm, and the thickness of the AlCl 3 The thickness of the patch material 3 is 2.5±0.5 mm, and the thickness of the gauze 2 is 1.5±0.5 mm. 4 ) 2 HPO 4The thickness of the patch material 4 is 2.5±0.5 mm, the thickness of the second agar spacer 6 is 5 mm, the thickness of the second buffer sponge 8 is 10 mm, and the size of the simulated weathering sample 1 wrapped by the gauze 2 is 20*20*10 mm.
[0064] During reinforcement, start the power supply 11, which is set to: current 30 mA, voltage 120 V; after the entire device is powered on for 24 hours, take out the rock cultural relics wrapped in gauze 2, rinse the reinforced samples with deionized water, and place them in a 55°C oven for 7 hours.
[0065] Comparative Example 1
[0066] A sample with the same source and the same degree of dissolution as the simulated weathering sample in Example 1 was selected without treatment as Comparative Example 1.
[0067] Comparative Example 2
[0068] Select samples with the same source and the same degree of dissolution as the simulated weathering specimens in Example 1, and add an aqueous solution of diammonium phosphate with a concentration of (0.1 to 0.2 M) and an aqueous solution of aluminum chloride with a concentration of (0.1 to 0.2 M) in sequence to the surface of the weathered carbonate rock cultural relics by drip infiltration for repair.
[0069] Performance Testing
[0070] The color difference detection process includes: using a portable colorimeter to test and record the L, a and b values of the sample surface. The CI E1976 color difference formula and its color rendering system CI ELAB are used to measure the color space of the object color. The color difference △E between two colors is the geometric distance between two positions in the CI E1976 (L, a, b) color space, calculated using the formula.
[0071] ΔE=[(ΔL) 2 +(Δa) 2 +(Δb) 2 ] 1 / 2 (1)
[0072] Wherein, △L=L sample-L standard; △a=a sample-a standard; △b=b sample-b standard.
[0073] Generally, △E is used to evaluate color difference. Smaller △E value indicates smaller color difference. During the experiment, 5 points were randomly selected from the sample for testing, and the average value was taken for analysis. The results are shown in Table 1.
[0074] Table 1
[0075]
[0076] Related studies have shown that when ΔE*<3 after reinforcement, the color change is not noticeable within the range that can be distinguished by the human eye; when ΔE* is between 3 and 5, the color difference between the materials is slightly different, which is within the generally acceptable range; when ΔE* is greater than 5, it is considered to be incompatible with aesthetic compatibility. In Example 1 of the present invention, the color difference values of the reinforced samples are all less than 3, indicating that the color change of the samples reinforced by the electrochemical method is within the acceptable range, and the color difference is 2.00.
[0077] The porosity testing process includes: testing the porosity of the hardened mortar using a MicroActive AutoPoreV 9600 mercury intrusion instrument according to ISO 15901 part 1. The results are shown in Table 2.
[0078] Table 2
[0079]
[0080] It can be seen that the porosity is reduced by 50.79% after reinforcement, indicating that the pores inside the sample are filled after reinforcement.
[0081] The acid resistance test process includes: drying the sample at 55°C to constant weight and weighing it; then preparing an acid solution with a pH of 3.5 using concentrated sulfuric acid and concentrated nitric acid in a molar ratio of 1:1, and the specific ratio is to add 5.43μL of concentrated sulfuric acid and 6.25μL of concentrated nitric acid to 1L of deionized water, wherein the concentration of concentrated sulfuric acid is 98%, and the concentration of concentrated nitric acid is 70%, both of which are produced by Sinopharm Group; then placing the sample in the acid solution, placing it in a 40Khz ultrasonic cleaning machine, shaking for 5h, taking out the sample and washing it with ultrapure water, drying it at 55°C for 18h, and weighing it, which is one cycle. The results after ten acid resistance cycles are shown in Table 3.
[0082] Table 3
[0083]
[0084] It can be seen from Table 3 that the mass loss rate of comparative example 1 after ten acid-resistant cycles is 2.10%, and the mass loss rate of embodiment 1 after ten acid-resistant cycles after electrochemical reinforcement is 0.12%. Compared with comparative example 1, the mass loss inhibition rate is as high as 94.28%. It can be seen that the acid-resistant effect is greatly improved after reinforcement.
[0085] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A device for reinforcing rock cultural relics, characterized in that: include: The electrochemical deposition cell comprises: an electrode connected to the positive electrode of a power source is arranged at one end of the electrochemical deposition cell, and an electrode connected to the negative electrode of the power source is arranged at the other end opposite thereto; The first buffer sponge, the first agar spacer, the AlCl3 application material, the weathered stone placement chamber, the (NH4)2HPO4 application material, the second agar spacer and the second buffer sponge are arranged between the two end electrodes in the electrochemical deposition cell, which are connected in sequence to form a conductive loop; The first buffer sponge and the second buffer sponge are soaked with phosphate buffer; The raw materials for preparing the AlCl3 patch material include cellulose and an AlCl3 aqueous solution with a concentration of 0.1 to 0.2 M, and the mass ratio of cellulose to the AlCl3 aqueous solution is 1:2 to 3; The raw materials for preparing the (NH4)2HPO4 patch material include cellulose and a (NH4)2HPO4 aqueous solution with a concentration of 0.1 to 0.2 M, and the mass ratio of cellulose to the (NH4)2HPO4 aqueous solution is 1:2 to 3; The outer wall of the weathered stone placement chamber is a porous material soaked in phosphate buffer solution, which is used to place the rock cultural relics to be reinforced.
2. The device for reinforcing rock cultural relics according to claim 1, characterized in that: The sponges in the first buffer sponge and the second buffer sponge are nano sponges.
3. The device for reinforcing rock cultural relics according to claim 1, characterized in that: Optionally, the phosphate buffer has a neutral pH value and includes potassium dihydrogen phosphate, sodium hydroxide and water.
4. The device for reinforcing rock cultural relics according to claim 3, characterized in that: In phosphate buffer, the concentration of potassium dihydrogen phosphate is 0.04-0.06M.
5. The device for reinforcing rock cultural relics according to claim 1, characterized in that: The raw materials for preparing the first agar spacer and the second agar spacer include agar and water in a mass ratio of (4-8):
96.
6. The device for reinforcing rock cultural relics according to claim 1, characterized in that: The porous material of the weathered stone placement room includes one or more of gauze, non-woven fabric and rice paper.
7. The device for reinforcing rock cultural relics according to claim 1, characterized in that: The rock cultural relics to be reinforced are made of carbonate rock.
8. The device for reinforcing rock cultural relics according to claim 1, characterized in that: The electrodes in the electrochemical deposition cell are connected to a power source via wires.
9. A method for reinforcing rock cultural relics using the device for reinforcing rock cultural relics according to any one of claims 1 to 8, characterized in that: Includes steps: Includes steps: S1. Wrap the rock cultural relics to be reinforced with porous materials, and immerse the porous materials in neutral phosphate buffer to obtain a weathered stone placement chamber; S2, AlCl3 patch material, a first agar pad and a first buffer sponge are sequentially connected to one side of the weathered stone material placement chamber; (NH4)2HPO4 patch material, a second agar pad and a second buffer sponge are sequentially connected to the other side of the weathered stone material placement chamber; S3. Connect the first buffer sponge to the positive pole of the power supply, connect the second buffer sponge to the negative pole of the power supply, start the power supply and maintain the set time to complete the reinforcement of the rock cultural relics.
10. The method for reinforcing rock cultural relics according to claim 9, characterized in that: In S3, the power supply settings are: current 30±5mA, voltage 120±10V; power-on time is 24±4h.
Citation Information
Patent Citations
Copper nanoparticle synthetic method using rolling circle amplification product as template and application thereof in electrochemical detection
CN105567808A
Dressing
CN110772378A
Aluminum phosphate double-modified high-nickel cobalt-free polycrystalline positive electrode material and preparation method thereof
CN117393739A
Coating concrete mouldings with glass or phosphate - by adding a salt to the concrete applying coating paste and curing
DE2539718A1
Process for the treatment of a calcium aluminophosphate
US4321244A