Modified aluminum powder and preparation method of zero-oxygen equilibrium core-shell composite energetic material containing modified aluminum powder
The RDX@Al/AP core-shell composite material was prepared by Fe2O3 coated aluminum powder and modified with perfluorododecium. The RDX@Al/AP core-shell composite material was prepared by combining with the Pickering emulsion method, which solved the problem of inconcentration of RDX and AP thermal decomposition in solid propellants, and achieved more efficient Energy release and combustion performance.
Patent Information
- Application Number
- CN202411071934.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The surface roughness of RDX, large internal defects of crystals and high temperature decomposition peak temperature of AP in existing solid propellants leads to inconcentration of energy release, affecting the ignition delay time, combustion rate and energy release performance. It is necessary to reduce the thermal decomposition temperature of AP through catalytic to Improve energy release efficiency.
采用Fe2O3包覆铝粉,并用全氟十二酸修饰Fe2O3包覆的铝粉,通过Pickering乳液法制备零氧平衡核壳复合含能材料,形成RDX@Al/AP结构,以催化AP的热分解 process and improve combustion performance.
It effectively reduces the thermal decomposition temperature of AP, improves the energy release rate and combustion performance, shortens the combustion time, and becomes more concentrated in energy release, significantly improves the thermal decomposition and combustion performance of composite materials, and improves safety performance.
Smart Images

Figure CN118908792A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of preparation of nonferrous aluminum materials and energetic materials, and more specifically, to a method for preparing a modified aluminum powder and a zero-oxygen balance core-shell composite energetic material containing the modified aluminum powder. Background Art
[0002] At present, solid propellant, as the main power source of rocket and missile engines, plays an important role in aerospace and modern missile technology. Many scholars have conducted a lot of research on it. The formula of solid propellant is mainly composed of binder, oxidizer, elemental metal combustion product and other functional agents. The performance of each component in the formula will affect the overall performance of solid propellant. Therefore, the formula selection of propellant system plays a decisive role in whether the performance of solid propellant is excellent.
[0003] As one of the common nitramine-based military explosives, RDX has the characteristics of strong explosive power and high energy density and is widely used as a high-energy filler in weapon systems and solid propellants. However, due to the rough surface, large internal defects and poor dispersibility of the current industrial-grade RDX, its application in weapon systems and solid propellants is greatly limited. So far, the strategy of modifying RDX is an effective strategy to solve this problem. The use of spheroidization, binder coating and other means to improve the performance of RDX has higher energy output and better safety performance; it has great research significance for the application of RDX. AP is the most widely used oxidant in solid propellants. Its thermal decomposition and combustion properties have a huge impact on the performance of solid propellants. However, due to the high temperature decomposition peak temperature of AP and the large temperature difference between the high and low temperature decomposition peaks, the heat release is not concentrated. As an important component in solid propellants, the thermal decomposition and combustion properties of AP play a vital role in the performance of the overall propellant. However, the current problem is that the high temperature decomposition peak temperature is high and the heat release is not concentrated, which in turn affects the ignition delay time, combustion rate and energy release performance of solid propellants. These problems need to be effectively solved to further improve the performance of solid propellants. Therefore, the thermal decomposition process of AP is catalyzed to reduce its thermal decomposition temperature, thereby improving thermal performance and making energy release more concentrated. Most of the existing studies use nano-metal powders or metal oxides as catalysts to reduce the decomposition temperature of AP and increase the combustion rate of AP. Some studies have used Al powder to catalyze the thermal decomposition process of AP, effectively reducing the activation energy of the AP thermal decomposition process, and the maximum reduction was 17.6%, while the reaction rate constant was increased by 32.5%; greatly improving the reaction rate and energy release efficiency of the AP thermal decomposition process. Zhou et al. used PDA as a bioadhesive and prepared two core-shell structure composites of Al@AP and Al@AP / CuO. Both composites effectively reduced the ignition delay time and achieved functionalization of controllable burning rate. It can be seen that adding metals or metal oxides to the solid propellant formula of AP can effectively promote the thermal decomposition performance and energy release rate of AP.
[0004] With the development of propellant systems, higher requirements are placed on the energy performance of solid propellants. Therefore, in order to further enhance the energy performance of solid propellants, adding metal powder to solid propellants is an effective strategy. Among them, nano-aluminum powder has attracted the attention of researchers because of its large specific surface area for reaction, small heat and mass transfer distance between components, and short ignition delay period. However, since the surface of Al powder is composed of Al2O3 shell, it will reduce the energy properties and limit its application. At present, some studies have used perfluorooctanoic acid (APFO) to corrode the surface shell of n-Al powder, which not only successfully reduced the apparent activation energy, but also successfully increased the energy output performance of n-Al. Different particles in nanocomposite combustion catalysts often interact with each other, thereby playing a certain catalytic role on other components in the propellant system. For composite energetic materials, the best morphology to improve the performance of the composite is to design a core-shell structure composite by integrating the components. The composite material with a core-shell structure can not only retain the excellent performance of the components themselves, but also promote the performance improvement of the composite material through the synergistic effect between the layers of components. Yan et al. used the Pickering emulsion method to prepare dodecylamine functionalized graphene (AmGO) as a surfactant, and prepared ADN@AmGO core-shell structure composite materials with ADN as the core, which had a significant thermal decomposition catalytic effect. Among them, Pickering emulsion has become a research hotspot due to its simple preparation, high stability and strong biocompatibility. In addition, since the Pickerin emulsion method uses nanoparticles as surfactants to link substances in the oil and water phases, it is no longer necessary to add other non-energetic component functional additives, reducing energy losses in the formula; this is very important for the formulation design of the propellant system. Summary of the invention
[0005] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0006] In order to achieve these purposes and other advantages according to the present invention, a modified aluminum powder is provided, characterized in that the aluminum powder is first coated with Fe2O3 to obtain the Fe2O3-coated aluminum powder, and then the Fe2O3-coated aluminum powder is modified with perfluorododecanoic acid.
[0007] A method for preparing modified aluminum powder comprises the following steps:
[0008] S11, coating aluminum powder with Fe2O3 to obtain Fe2O3-coated aluminum powder;
[0009] S12, dissolving perfluorododecanoic acid in ethyl acetate, and dispersing Fe2O3-coated aluminum powder in cyclohexane;
[0010] S13. Under magnetic stirring, slowly drop ethyl acetate containing perfluorododecanoic acid into cyclohexane containing Fe2O3-coated aluminum powder, then continue stirring to react, filter, wash with cyclohexane several times, and put in an oven to dry for 2 to 6 hours to obtain modified aluminum powder.
[0011] Preferably, in S11, the specific method of coating aluminum powder with Fe2O3 includes: adding ammonia water to a 0.1-0.5 mol / L ferric nitrate solution and stirring, and when a precipitate is generated, continuing stirring and adding aluminum powder and polyoxyethylene ether, ultrasonically oscillating at a frequency of 50-120 kHz for 10-20 min, standing and aging for 6-24 h, and then separating the solid and liquid, washing the separated solid powder, and vacuum freeze-drying it, and then heating it to 500-900°C at a heating rate of 2-4°C / min in an argon atmosphere, calcining it for 1-3 h, and obtaining Fe2O3-coated aluminum powder; wherein the mass ratio of ferric nitrate and ammonia water is 1:1-2, and the mass ratio of the mass of aluminum powder, ammonia water, and polyoxyethylene ether is 2-3:1:0.05-0.2.
[0012] Preferably, in S12, the mass volume ratio of perfluorododecanoic acid, ethyl acetate, aluminum powder and cyclohexane is 0.01 g:10-30 mL:1 g:100-300 mL.
[0013] Preferably, in S13, the magnetic stirring speed is 200 to 600 rpm; and the stirring reaction time is 1 to 3 h.
[0014] A method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder comprises: adding cyclotrimethylene trinitramine into a solvent and ultrasonically dissolving the material to obtain a cyclotrimethylene trinitramine solution; dissolving ammonium perchlorate in water to obtain an ammonium perchlorate solution, dripping the ammonium perchlorate solution into the cyclotrimethylene trinitramine solution, ultrasonically treating the material, adding modified aluminum powder, ultrasonically treating the material again, standing the material and performing vacuum freeze drying to obtain a zero oxygen balance core-shell composite energetic material Zero-EM-RDX@Al / AP.
[0015] Preferably, the solvent is ethyl acetate.
[0016] Preferably, the mass volume ratio of cyclotrimethylene trinitramine, solvent, ammonium perchlorate, water and modified aluminum powder is 0.1-0.15 g: 2-6 mL: 0.05-0.1 g: 2-16 mL: 0.01-0.3 g.
[0017] Preferably, the ultrasonic time after cyclotrimethylene trinitramine is added to the solvent is 4 to 10 minutes;
[0018] The ultrasonic time after the ammonium perchlorate solution is added dropwise into the cyclotrimethylene trinitramine solution is 1 to 5 minutes;
[0019] The ultrasonic time after adding the modified aluminum powder is 5 to 15 minutes, and the standing time is 0 to 40 minutes.
[0020] A zero oxygen balance core-shell composite energetic material containing modified aluminum powder, comprising:
[0021] The inner core is made of cyclotrimethylene trinitramine;
[0022] The outer shell is coated on the outside of the inner core, and the outer shell is a composite material of modified aluminum powder and ammonium perchlorate.
[0023] The present invention has at least the following beneficial effects:
[0024] The invention first coats the aluminum powder with Fe2O3 before using perfluorododecanoic acid to modify the aluminum powder to obtain Fe2O3-coated aluminum powder, then uses perfluorododecanoic acid to modify the Fe2O3-coated aluminum powder, and finally prepares the zero oxygen balance core-shell composite energetic material by a Pickering emulsion method; in the process of Fe2O3 coating, polyoxyethylene ether is used as a dispersant to reduce the agglomeration between the aluminum powders, so that Fe2O3 is evenly coated on the surface of the aluminum powder, and the compactness of the Fe2O3 coating on the aluminum powder is improved; Fe2O3 coating on the aluminum powder improves the energy release rate and combustion performance of the zero oxygen balance core-shell composite energetic material, and the energy release is more concentrated.
[0025] Based on the multiple advantages of core-shell structure in the field of energetic materials, the present invention designs a composite material with RDX as the core and composite particles of aluminum and ammonium perchlorate (AP) as the shell. The surface activity and hydrophilic and lipophilic properties of aluminum powder modified by perfluorododecanoic acid are changed; the RDX@Al / AP core-shell structure composite is prepared by Pickering emulsion method. The optimal conditions for emulsion stability are determined as follows: oil-water volume ratio of 2:5, 20wt% modified Al powder, and standing time within 20min.
[0026] (1) Thermal performance tests show that the zero-oxygen-balanced RDX@Al / AP prepared by the Pickering emulsion method can not only catalyze the thermal decomposition process of the raw materials RDX and AP, but also the catalytic effect on the thermal decomposition process of AP becomes more significant as the proportion of Al powder increases.
[0027] (2) The combustion test shows that compared with the physical mixed samples, the combustion time of the zero oxygen balance RDX@Al / AP composite material prepared by the Pickering emulsion method is shortened from 1473ms to 540ms, with faster combustion, concentrated energy release time, and shorter heat and mass transfer distance between components. This fully demonstrates that the core-shell composite energetic material using the zero oxygen balance ratio can effectively improve the energy release rate and efficiency, and fully demonstrates the advantage of the high energy level density of the composite energetic material. At the same time, with the increase of Al powder content, the combustion time is shorter and the combustion process is more violent; especially when the Al powder accounts for 20wt%, the RDX@Al / AP sample exhibits deflagration.
[0028] (3) The sensitivity test results show that compared with the raw material RDX, the H 50 The increase from 14.49cm to 24.29cm improves the composite material's performance in resisting impact sensitivity; however, due to factors such as the rough surface of the composite, its friction sensitivity is slightly increased. Without adding non-energetic additives, the use of solid particle surfactants can effectively ensure the energy performance of the composite material. Based on the design of zero oxygen balance ratio, the prepared core-shell structured energetic composite material can not only give full play to the excellent performance of each component, but also effectively improve the energy release performance, thereby improving the thermal decomposition performance and combustion performance of the composite material. At the same time, the morphological advantages of the core-shell structure improve the safety performance of the composite energetic material, which is an effective strategy for the preparation of high-performance composite materials with core-shell structure by Pickering emulsion method, and provides a way of thinking for the application of RDX / Al-based composite materials in solid propellants.
[0029] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The raw materials Al, perfluorodecanoic acid and modified Al powder in Comparative Example 1 of the present invention are 400-3000 cm -1 FT-IR spectra within the range;
[0031] Figure 2 The SEM images of the raw material RDX, modified Al powder, AP and Zero-EM-RDX@Al / AP in Comparative Example 1;
[0032] Figure 3 The SEM image and surface element distribution map of Zero-EM-RDX@Al / AP prepared in Comparative Example 1;
[0033] Figure 4XRD spectra of Zero-EM-RDX@Al / AP, modified Al powder and AP prepared in Comparative Example 1;
[0034] Figure 5 FT-IR spectra of Zero-EM-RDX@Al / AP, modified Al, AP and RDX prepared in Comparative Example 1;
[0035] Figure 6 TG-DSC curve of Mix sample prepared by physical mixing method in Comparative Example 18;
[0036] Figure 7 TG-DSC curve of Zero-EM-RDX@Al / AP prepared in Comparative Example 1;
[0037] Figure 8 DSC curves of the raw materials RDX and AP in Comparative Example 1;
[0038] Fig. 9 TG curves of the raw materials RDX and AP in Comparative Example 1;
[0039] Fig.10 DSC curves of Zero-EM-RDX@Al / AP prepared in Comparative Examples 1 to 3;
[0040] Fig.11 TG curves of Zero-EM-RDX@Al / AP prepared in Comparative Examples 1 to 3;
[0041] Fig.12 It is a comparison chart of the combustion performance test of Zero-EM-RDX@Al / AP prepared in Comparative Example 1 and the Mix sample prepared in Comparative Example 18;
[0042] Fig.13 This is a comparison chart of the combustion performance tests of Zero-EM-RDX@Al / AP prepared in Comparative Examples 1 to 3;
[0043] Fig.14 This is a comparison chart of the impact sensitivity and friction sensitivity of Zero-EM-RDX@Al / AP prepared in Comparative Example 1 and the raw material RDX;
[0044] Fig.15 These are microscopic images of the Pickering emulsions prepared in Comparative Examples 5 to 17 and 19. DETAILED DESCRIPTION
[0045] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0046] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0047] Example 1
[0048] This embodiment provides a method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, comprising the following steps:
[0049] Step 1: Prepare modified aluminum powder. The specific steps are:
[0050] S11. Al powder is first coated with Fe2O3 to obtain Al powder coated with Fe2O3. The specific method includes: adding 0.34g of ammonia water to 50mL of 0.2mol / L ferric nitrate solution, and stirring. When a precipitate is generated, continue stirring and add 0.68g of Al powder and 0.068g of polyoxyethylene ether, ultrasonically oscillate at a frequency of 60kHZ for 20min, stand and age for 12h, then separate the solid and liquid, wash the separated solid powder, and vacuum freeze-dry it, then heat it to 600°C at a heating rate of 2°C / min in an argon atmosphere, and calcine it for 2h to obtain Fe2O3-coated Al powder.
[0051] S12, dissolve 0.01 g of perfluorododecanoic acid in 20 mL of ethyl acetate, and disperse 1 g of Fe2O3-coated Al powder in 200 mL of cyclohexane;
[0052] S13. Under magnetic stirring at 300 rpm, slowly drop ethyl acetate containing perfluorododecanoic acid into cyclohexane containing Al powder coated with Fe2O3, then continue stirring to react for 1 hour, filter, wash with cyclohexane several times, and put in an oven to dry for 3 hours to obtain modified Al powder.
[0053] Step 2: Add 0.1 g of cyclotrimethylene trinitramine (RDX) to a beaker containing 4 mL of ethyl acetate and ultrasonicate for 5 minutes to obtain a cyclotrimethylene trinitramine solution; dissolve 0.09 g of ammonium perchlorate (AP) in a beaker containing 10 mL of water to obtain an ammonium perchlorate solution, add the ammonium perchlorate solution dropwise into the cyclotrimethylene trinitramine solution, ultrasonicate, add 0.01 g of modified Al powder, ultrasonicate again for 10 minutes, stand for 20 minutes, and then perform vacuum freeze-drying to obtain a zero oxygen balance core-shell composite energetic material Zero-EM-RDX@Al / AP with cyclotrimethylene trinitramine as the core and a composite material of modified Al powder and ammonium perchlorate as the shell.
[0054] Example 2
[0055] This embodiment provides a method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, comprising the following steps:
[0056] Step 1: preparing modified aluminum powder, the specific steps are:
[0057] S11. Al powder is first coated with Fe2O3 to obtain Al powder coated with Fe2O3. The specific method includes: adding 0.68g of ammonia water to 80mL of 0.5mol / L ferric nitrate solution, and stirring. When a precipitate is generated, continue stirring and add 2.04g of Al powder and 0.2g of polyoxyethylene ether, ultrasonically oscillate at a frequency of 120kHZ for 20min, stand and age for 12h, then separate the solid and liquid, wash the separated solid powder, and vacuum freeze-dry it, then heat it to 800°C at a heating rate of 4°C / min in an argon atmosphere, and calcine it for 2h to obtain Fe2O3-coated Al powder.
[0058] S12, dissolve 0.01 g of perfluorododecanoic acid in 20 mL of ethyl acetate, and disperse 1 g of Fe2O3-coated Al powder in 200 mL of cyclohexane;
[0059] S13. Under magnetic stirring at 300 rpm, slowly drop ethyl acetate containing perfluorododecanoic acid into cyclohexane containing Al powder coated with Fe2O3, then continue stirring to react for 1 hour, filter, wash with cyclohexane several times, and put in an oven to dry for 3 hours to obtain modified Al powder.
[0060] Step 2: Add 0.1 g of cyclotrimethylene trinitramine (RDX) to a beaker containing 4 mL of ethyl acetate and ultrasonicate for 5 minutes to obtain a cyclotrimethylene trinitramine solution; dissolve 0.09 g of ammonium perchlorate (AP) in a beaker containing 10 mL of water to obtain an ammonium perchlorate solution, add the ammonium perchlorate solution dropwise into the cyclotrimethylene trinitramine solution, ultrasonicate, add 0.01 g of modified Al powder, ultrasonicate again for 10 minutes, stand for 20 minutes, and then perform vacuum freeze-drying to obtain a zero oxygen balance core-shell composite energetic material Zero-EM-RDX@Al / AP with cyclotrimethylene trinitramine as the core and a composite material of modified Al powder and ammonium perchlorate as the shell.
[0061] Comparative Example 1
[0062] This comparative example provides a method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, comprising the following steps:
[0063] Step 1: using perfluorododecanoic acid to modify Al powder to prepare modified Al powder, the specific method includes:
[0064] S11, dissolve 0.01 g of perfluorododecanoic acid in 20 mL of ethyl acetate, and disperse 1 g of Al powder in 200 mL of cyclohexane;
[0065] S12. Under magnetic stirring at 300 rpm, slowly drop ethyl acetate containing perfluorododecanoic acid into cyclohexane containing Al powder, then continue stirring to react for 1 hour, filter, wash with cyclohexane several times, and put in an oven to dry for 3 hours to obtain modified Al powder.
[0066] Step 2: Add 0.1g of cyclotrimethylene trinitramine (RDX) to a beaker containing 4mL of ethyl acetate and ultrasonicate for 5min to obtain a cyclotrimethylene trinitramine solution; dissolve 0.09g of ammonium perchlorate (AP) in a beaker containing 10mL of water to obtain an ammonium perchlorate solution, drop the ammonium perchlorate solution into the cyclotrimethylene trinitramine solution, ultrasonicate, add 0.01g of modified Al powder, ultrasonicate again for 10min, stand for 20min and then perform vacuum freeze drying to obtain a zero oxygen balance core-shell composite energetic material Zero-EM-RDX@Al / AP with cyclotrimethylene trinitramine as the core and a composite material of modified Al and ammonium perchlorate as the shell. The zero oxygen balance core-shell composite energetic material Zero-EM-RDX@Al / AP prepared in this comparative example is recorded as 1%-EM-RDX@Al / AP.
[0067] Comparative Example 2
[0068] This comparative example provides a method for preparing a zero-oxygen balance core-shell composite energetic material containing modified aluminum powder. The difference from comparative example 1 is that the mass of the modified Al powder added in step 2 is 0.1 g, and the rest of the process methods are the same as those in comparative example 1. The zero-oxygen balance core-shell composite energetic material Zero-EM-RDX@Al / AP prepared in this comparative example is 10%-EM-RDX@Al / AP.
[0069] Comparative Example 3
[0070] This comparative example provides a method for preparing a zero-oxygen balance core-shell composite energetic material containing modified aluminum powder. The difference from comparative example 1 is that the mass of the modified Al powder added in step 2 is 0.2 g, and the rest of the process methods are the same as those in comparative example 1. The zero-oxygen balance core-shell composite energetic material Zero-EM-RDX@Al / AP prepared in this comparative example is 20%-EM-RDX@Al / AP.
[0071] Comparative Example 4
[0072] This comparative example provides a method for preparing a zero-oxygen balance core-shell composite energetic material containing modified aluminum powder. The difference from comparative example 1 is that the mass of the modified Al powder added in step 2 is 0.3 g, and the rest of the process methods are the same as those in comparative example 1.
[0073] Comparative Example 5
[0074] The present comparative example provides a method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, wherein step one is the same as comparative example 1, except that step two is: adding 0.08 g of cyclotrimethylene trinitramine (RDX) into a beaker containing 6 mL of ethyl acetate and ultrasonicating for 5 min to obtain a cyclotrimethylene trinitramine solution; dissolving 0.06 g of ammonium perchlorate (AP) in a beaker containing 2 mL of water to obtain an ammonium perchlorate solution, and dropping the ammonium perchlorate solution into the cyclotrimethylene trinitramine solution, ultrasonicating, adding 0.01 g of modified Al powder, ultrasonicating again for 10 min, standing for 20 min, and then vacuum freeze-drying to obtain a zero oxygen balance core-shell composite energetic material.
[0075] Comparative Example 6
[0076] The present comparative example provides a method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, wherein step one is the same as comparative example 1, except that step two is: adding 0.08 g of cyclotrimethylene trinitramine (RDX) into a beaker containing 6 mL of ethyl acetate and ultrasonicating for 5 min to obtain a cyclotrimethylene trinitramine solution; dissolving 0.06 g of ammonium perchlorate (AP) in a beaker containing 6 mL of water to obtain an ammonium perchlorate solution, dropping the ammonium perchlorate solution into the cyclotrimethylene trinitramine solution, ultrasonicating, adding 0.01 g of modified Al powder, ultrasonicating again for 10 min, standing for 20 min, and then vacuum freeze-drying to obtain a zero oxygen balance core-shell composite energetic material.
[0077] Comparative Example 7
[0078] The present comparative example provides a preparation method of a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, wherein step 1 is the same as comparative example 1, except that step 2 is: adding 0.08 g of cyclotrimethylene trinitramine (RDX) into a beaker containing 4 mL of ethyl acetate and ultrasonicating for 5 min to obtain a cyclotrimethylene trinitramine solution; dissolving 0.06 g of ammonium perchlorate (AP) in a beaker containing 10 mL of water to obtain an ammonium perchlorate solution, dropping the ammonium perchlorate solution into the cyclotrimethylene trinitramine solution, ultrasonicating, adding 0.01 g of modified Al powder, ultrasonicating again for 10 min, standing for 20 min and then performing vacuum freeze drying to obtain a zero oxygen balance core-shell composite energetic material.
[0079] Comparative Example 8
[0080] The present comparative example provides a method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, wherein step 1 is the same as comparative example 1, except that step 2 is: 0.08 g of cyclotrimethylene trinitramine (RDX) is added to a beaker containing 2 mL of ethyl acetate and ultrasonicated for 5 min to obtain a cyclotrimethylene trinitramine solution; 0.06 g of ammonium perchlorate (AP) is dissolved in a beaker containing 6 mL of water to obtain an ammonium perchlorate solution, the ammonium perchlorate solution is added dropwise to the cyclotrimethylene trinitramine solution, ultrasonicated, 0.01 g of modified Al powder is added, ultrasonicated again for 10 min, and vacuum freeze-dried after standing for 20 min to obtain a zero oxygen balance core-shell composite energetic material.
[0081] Comparative Example 9
[0082] The present comparative example provides a method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, wherein step 1 is the same as comparative example 1, except that step 2 is: adding 0.08 g of cyclotrimethylene trinitramine (RDX) to a beaker containing 2 mL of ethyl acetate and ultrasonicating for 5 min to obtain a cyclotrimethylene trinitramine solution; dissolving 0.06 g of ammonium perchlorate (AP) in a beaker containing 10 mL of water to obtain an ammonium perchlorate solution, and dropping the ammonium perchlorate solution into the cyclotrimethylene trinitramine solution, ultrasonicating, adding 0.01 g of modified Al powder, ultrasonicating again for 10 min, standing for 20 min, and then vacuum freeze-drying to obtain a zero oxygen balance core-shell composite energetic material.
[0083] Comparative Example 10
[0084] The present comparative example provides a method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, wherein step one is the same as comparative example 1, except that step two is: adding 0.08 g of cyclotrimethylene trinitramine (RDX) into a beaker containing 2 mL of ethyl acetate and ultrasonicating for 5 min to obtain a cyclotrimethylene trinitramine solution; dissolving 0.06 g of ammonium perchlorate (AP) in a beaker containing 16 mL of water to obtain an ammonium perchlorate solution, and dropping the ammonium perchlorate solution into the cyclotrimethylene trinitramine solution, ultrasonicating, adding 0.01 g of modified Al powder, ultrasonicating again for 10 min, standing for 20 min, and then vacuum freeze-drying to obtain a zero oxygen balance core-shell composite energetic material.
[0085] Comparative Example 11
[0086] This comparative example provides a method for preparing a zero-oxygen balance core-shell composite energetic material based on modified aluminum powder, wherein step 1 is the same as comparative example 7, except that the amount of modified Al powder used in step 2 is 0.1 g, and the other method parameters are the same as those of comparative example 7.
[0087] Comparative Example 12
[0088] This comparative example provides a method for preparing a zero oxygen equilibrium core-shell composite energetic material containing modified aluminum powder, wherein step one is the same as comparative example 7, except that the amount of modified Al powder used in step two is 0.2 g, and the other method parameters are the same as those in comparative example 7.
[0089] Comparative Example 13
[0090] This comparative example provides a method for preparing a zero-oxygen equilibrium core-shell composite energetic material containing modified aluminum powder, wherein step one is the same as comparative example 7, except that the amount of modified Al powder used in step two is 0.3 g, and the other method parameters are the same as those of comparative example 7.
[0091] Comparative Example 14
[0092] This comparative example provides a method for preparing a zero-oxygen equilibrium core-shell composite energetic material containing modified aluminum powder, wherein step one is the same as comparative example 12, except that no standing is performed in step two.
[0093] Comparative Example 15
[0094] This comparative example provides a method for preparing a zero-oxygen equilibrium core-shell composite energetic material containing modified aluminum powder, wherein step 1 is the same as comparative example 12, except that the standing time in step 2 is 10 minutes.
[0095] Comparative Example 16
[0096] This comparative example provides a method for preparing a zero-oxygen equilibrium core-shell composite energetic material containing modified aluminum powder, wherein step 1 is the same as comparative example 12, except that the standing time in step 2 is 30 minutes.
[0097] Comparative Example 17
[0098] This comparative example provides a method for preparing a zero-oxygen equilibrium core-shell composite energetic material containing modified aluminum powder, wherein step one is the same as comparative example 12, except that the standing time in step two is 40 minutes.
[0099] Comparative Example 18
[0100] In this comparative example, 0.1 g of cyclotrimethylene trinitramine, 0.09 g of ammonium perchlorate and 0.01 g of modified Al powder (the modification method of the modified Al is the same as that of comparative example 1) are mixed to obtain a Mix sample.
[0101] Comparative Example 19
[0102] This comparative example provides a method for preparing a zero-oxygen equilibrium core-shell composite energetic material containing modified aluminum powder. The difference from comparative example 5 is that 0.2 g of unmodified Al powder is used to replace the modified Al powder in step 2, and the other method parameters are the same as those in comparative example 5.
[0103] The most important thing when preparing samples using the emulsion method is the stability of the emulsion, because the stability of the emulsion will affect the final microscopic morphology of the prepared composite, the size of the particles, the degree of coating, etc., and thus affect the performance of the composite. For Comparative Examples 5 to 17 and 19, under the condition that the mass ratio of RDX to AP is 4:3, the oil-water ratio, the content of modified nano-aluminum, and the standing time of the Pickering emulsion are explored to infer the influence of various influencing factors on the stability of the emulsion. A digital video polarizing microscope (ZOOM-620E) was used to observe the images of the Pickering emulsion under different conditions. The characterization results are shown in Figure 1. Fig.15 shown.
[0104] Fig.15 (a) shows the emulsion image of unmodified aluminum powder. Fig.15 (b) to (g) correspond to comparative examples 5 to 10, i.e., emulsion images with a modified aluminum powder content of 1 wt% and an oil-water volume ratio of 3:1, 1:1, 2:5, 1:3, 1:5, and 1:8. Fig.15 As can be seen from (a), there is an obvious stratification phenomenon between the oil and water phases of the emulsion prepared by the Al powder that has not been modified with perfluorododecanoic acid, and since ethyl acetate has a lower density than water, it floats on the upper layer, and Al particles are distributed in both the oil and water phases; and the microscopic image shows a disordered particle distribution without spherical droplets. Fig.15 The results of (b) to (g) show that when the oil-water volume ratio is 3:1, there are floating Al particles in the emulsion, spherical droplets of different sizes are in close contact, and the emulsion is stratified. When the oil-water volume ratio is 1:1, the size of the spherical droplets in close contact decreases, and the emulsion is stratified; when the oil-water volume ratio is 2:5, the microscopic image of the emulsion has spherical droplets of uniform size and good dispersion, and the emulsion is not stratified. When the oil-water volume ratio is increased to 1:3, scattered solid particles appear in the emulsion, and the emulsion is stratified. When the oil-water volume ratio is further increased to 1:5 and 1:8, it can be found that the spherical droplets basically disappear, the emulsion is stratified, and the microscopic image shows that crystals of explosives are precipitated. Because ethyl acetate is also slightly soluble in the aqueous phase system, explosive crystals are precipitated from the oil phase system.
[0105] Fig.15(h) to (k) correspond to Comparative Example 7, Comparative Example 11-Comparative Example 13, respectively, and represent the emulsion images of modified aluminum powder with 1wt%, 10wt%, 20wt%, and 30wt% added under the condition of oil-water volume ratio of 2:5. It can be found that modified aluminum powders of different mass ratios can form stable emulsions, and there is a layer of solid particle film on the surface of the droplets, so that the oil phase droplets can stably exist in the water phase. With the increase of the proportion of modified aluminum powder, it is found that the solid particle film of the oil phase droplets gradually increases until the aluminum powder proportion reaches 20wt% to form uniformly sized dispersed black spherical droplets. When the proportion of modified Al powder increases to 30wt%, it is found that the spherical droplets are of different sizes, and solid particles and large agglomerates appear. Mainly due to the excessive solid surfactant, the nano-modified Al powder cannot be dispersed in the emulsion, and agglomerates are formed under the action of ultrasonic oscillation.
[0106] Fig.15 (l) to (p) correspond to Comparative Example 14, Comparative Example 15, Comparative Example 12, Comparative Example 16 and Comparative Example 17, respectively, showing the microscopic images of the prepared emulsions with a standing time of 0 min, 10 min, 20 min, 30 min and 40 min under the conditions of a modified aluminum powder ratio of 20 wt% and an oil-water ratio of 2:5. It can be seen from the figure that the emulsion has no stratification when the standing time is 20 min. When the standing time is 30 min, although the emulsion has no obvious stratification phenomenon, the microscopic image shows that crystals are precipitated at 30 min, and the number of spherical droplets is greatly reduced. When the standing time reaches 40 min, the emulsion shows obvious stratification, all the explosive crystals are precipitated, and the spherical droplets completely disappear. The reason for this phenomenon is that the water phase and the oil phase have different densities. As the standing time increases, the spherical droplets of the oil phase gradually move upward due to their low density, and the droplets collide and merge to form large droplets. The surface film formed by the modified Al powder breaks during the collision and fusion process, and explosives precipitate. At the same time, the perfluorododecanoic acid on the surface of the modified Al powder will also dissolve in water, reducing the surface activity and amphiphilicity of the Al powder, resulting in the rupture of the emulsion and stratification.
[0107] The main reason for using perfluorodecanoic acid to modify Al powder is that the CF bond on the carbon chain of perfluorodecanoic acid has good lipophilicity, which can adjust the surface tension of Al powder, making the Al surface highly active and acting as a surfactant molecule to form Pickering emulsion. Therefore, whether the modified Al powder has a functional group containing a CF bond becomes an important judgment factor. In order to prove whether perfluorodecanoic acid has successfully modified Al powder, FT-IR was used to test and analyze the functional groups of the modified samples, and the test results were characterized as follows: Figure 1As shown. Perfluorododecanoic acid activates Al powder mainly by reacting with Al2O3 on the Al surface, so perfluorododecanoic acid will not cause Al to carry other groups. Compared with the raw Al powder, the FT-IR graph of the modified Al is between 1000-1500cm -1 The range changes, corresponding to 1153cm -1 The symmetrical stretching vibration peak of the C-F bond at 1205 cm -1 The asymmetric stretching vibration peak of the CF bond at 1 is shown in Figure 2. This proves that the perfluorododecanoic acid has successfully modified the Al powder and changed the surface activity of Al, making preliminary preparations for the preparation of the Pickering emulsion system.
[0108] The morphology and structure of the raw material RDX, AP, modified Al powder and the zero oxygen balance core-shell composite energetic material Zero-EM-RDX@Al / AP prepared in Comparative Example 1 were characterized by SEM. Figure 2 As shown, Figure 2 (a) is the morphology of raw material RDX, (b) is the morphology of modified Al powder, (c) is the morphology of AP, and (d) is the morphology of zero oxygen equilibrium core-shell composite energetic material Zero-EM-RDX@Al / AP. The crystal size of RDX is about 80μm, the particle size of raw material Al powder is about 60-100nm, and the size of raw material AP is about 120μm. The particle size of Zero-EM-RDX@Al / AP composite sample is about 20μm, the particle surface is rough, and it is completely covered by a layer of dense particles. There are spherical small particles, smooth irregular crystals and similar composite particles on the rough surface of the composite sample. Combined with the molding mechanism of Pickering emulsion method and literature research, it is speculated that the Al powder modified with perfluorododecanoic acid is dispersed on the surface of ethyl acetate droplets of RDX, because its amphiphilicity attracts AP water droplets to form a water-in-oil structure of Pickering emulsion. During the vacuum drying process, since the volume of the water phase is much larger than that of the oil phase, as the oil-water phase decreases, the RDX in the oil phase first precipitates crystals to form a core. At the same time, the AP in the water phase recrystallizes and forms composite particles with the modified Al powder, which are coated on the surface of the RDX recrystallized body to form Zero-EM-RDX@Al / AP core-shell composite materials. In order to verify this conclusion, EDS was used to characterize and analyze the surface element composition and element distribution of the composite sample prepared by Pickering emulsion to determine the composition of the surface material.
[0109] At the same time, energy dispersive spectroscopy (EDS) was used to analyze and characterize the surface element distribution of the composite material. The characterization results are as follows: Figure 3 As shown, from Figure 3It was found that the surface elements of the composite sample prepared by Pickering emulsion were distributed with five elements: C, N, O, Al, and Cl. Since Cl is a unique elemental composition of AP, it can be shown that the dense coating layer on the surface of the composite is composed of composite particles of Al and AP, confirming the above speculation. Therefore, it can be considered that the Zero-EM-RDX@Al / AP core-shell composite material with Al / AP as the shell layer was prepared by Pickering emulsion technology.
[0110] The Zero-EM-RDX@Al / AP core-shell composite material, raw material RDX, AP and modified Al were characterized and tested by X-ray diffractometer. The results are as follows Figure 4 As shown. From the XRD diagram, it can be found that the characteristic diffraction peaks of the raw material RDX are basically consistent with the characteristic peaks of the RDX@Al / AP complex, proving that the crystal form of RDX has not changed during the preparation and recrystallization process. The new characteristic peak 2θ values in the complex are 38.4°, 44.6°, 64.9° and 19.3°, 23.8°, 27.4°. These diffraction peaks correspond to the diffraction values of (111), (200), (220) in the n-Al face-centered cubic structure and the crystal plane diffraction values of (101), (201), (211) of AP, respectively, corresponding to the raw material AP and the modified Al. It proves that the crystal form of AP has not changed during the recrystallization process and no chemical changes have occurred between the components.
[0111] Figure 5 The FT-IR images of raw material RDX, raw material AP, modified n-Al and Zero-EM-RDX@Al / AP core-shell composite materials are shown. From the figure, it can be found that the characteristic diffraction peak shape of Zero-EM-RDX@Al / AP core-shell composite material is basically consistent with that of raw material RDX, reflecting the typical absorption vibration peak shape of RDX. Secondly, AP at 621cm -1 The bending vibration peak of the OH bond appears at 1083cm -1 The characteristic absorption peak of ClO-4 appears at 1402cm -1 The stretching vibration absorption peak of the NH bond appears at 1153 cm -1 The symmetrical stretching vibration peak of the C-F bond and 1205 cm -1The asymmetric stretching vibration peak of the CF bond appears in the infrared characteristic diffraction peak of the Zero-EM-RDX@Al / AP core-shell composite material, which proves that AP and modified Al powder appear in the composite. Combined with the molding mechanism of the Pickering emulsion method and the analysis and test results of SEM, EDS, and XRD, it is inferred that the Pickering emulsion method was successfully used to prepare a composite material with RDX as the core and Al / AP composite particles as the shell.
[0112] In order to better understand the thermal decomposition performance of the samples, the physical mixing method was used to prepare the samples (Mix sample) and the Pickering emulsion method was used to prepare Zero-EM-RDX@Al / AP according to the zero oxygen balance mass ratio (RDX:AP:Al=10:9:1). The thermal decomposition process of the samples prepared by different methods was studied and analyzed by TG-DSC at a heating rate of 20℃ / min in a nitrogen atmosphere. The results are as follows: Figure 6 , Figure 7 At the same time, the raw materials RDX and AP were also tested and characterized under the same conditions. The results are shown in Figure 8 , Fig. 9 shown.
[0113] Combination Figure 6 , Figure 7 and Figure 8 , Fig. 9 It can be found that the physically mixed samples have three independent exothermic stages. The first stage is consistent with the thermal decomposition process of RDX. The peak temperature of the endothermic melting peak has almost no change, but the exothermic peak of the raw material RDX is advanced from 258.3℃ to 220.5℃, 37.8℃ in advance. The second stage is consistent with the low-temperature decomposition stage of the raw material AP. First, AP absorbs heat at 250.5℃, and the crystal form of AP is transformed from orthorhombic to cubic. Partial decomposition occurs at 318.3℃, and some gas products are generated; the third stage is the high-temperature exothermic stage of AP. At 406.6℃, AP is completely decomposed, and gas products and a large amount of heat are released. The TG weight loss curve is consistent with the DSC thermal decomposition curve, and is also divided into three stages corresponding to the thermal decomposition of RDX, the low-temperature decomposition stage of AP, and the high-temperature decomposition stage of AP.
[0114] Combination Figure 6 , Figure 7 and Fig. 9It can be found that although the EM-RDX@Al / AP sample prepared by the Pickering emulsion method still has three independent exothermic stages in the DSC exothermic curve, the TG thermal weight loss curve has only two weight loss stages. And compared with the mixed sample, the low-temperature decomposition peak of AP changes from 318.3℃ to 323.7℃, which is within the error range and the change is negligible. The peak temperature of the high-temperature decomposition peak changes from 406.6℃ to 386.9℃. The main reason for this phenomenon is related to the unique morphology and structure of the Zero-EM-RDX@Al / AP sample. Because AP and Al particles are coated on the surface of RDX in the form of composite particles, and the Al2O3 shell layer on the n-Al surface has a certain catalytic effect on the high-temperature decomposition stage of AP, it will advance the peak temperature of the high-temperature decomposition peak by 19.7℃. RDX first decomposes in the shell layer to release heat, which will promote the low-temperature thermal decomposition process of AP during the heat transfer process, so that the TG curve of the EM-RDX@Al / AP sample has only two thermal weight loss processes. At the same time, this conclusion can also be indirectly confirmed by the fact that the peak temperature of the AP high-temperature decomposition peak of the mixed sample has not changed.
[0115] In order to further study the effect of Al powder content on the thermal decomposition performance of RDX@Al / AP composite samples prepared by Pickering emulsion method, three core-shell structure composite samples of 1%-EM-RDX@Al / AP, 10%-EM-RDX@Al / AP, and 20%-EM-RDX@Al / AP with Al powder mass ratios of 1wt%, 10wt%, and 20wt% were prepared by Pickering emulsion method under the premise of mass ratio (RDX:AP=10:9). Under the same test conditions as above, the changes in DSC and TG curves of the three composite samples were observed, and their thermal decomposition performance was analyzed and studied. The test results are shown in the figure. Fig.10 and Fig.11 Combined with the above test results, Fig.10It can be found from the DSC curve that the thermal decomposition process of the composite is still three stages, and the TG curve shows two thermal weight loss stages. With the increase of the content of modified Al powder, the peak temperature of the high temperature decomposition peak of AP is further advanced, from 399.3℃ to 380.9℃ and then to 372.2℃. It proves that with the increase of the content of composite Al powder, it will further catalyze the thermal decomposition of AP. Compared with the mixed sample, the RDX@Al / AP composite prepared by the Pickering emulsion method advances the peak temperature of the high temperature decomposition peak of AP by 34.4℃ at most, further proving that the Al particles prepared by simple physical mixing have no catalytic effect on the thermal decomposition of AP, but the composite of Al and AP in the shell layer by the Pickering emulsion method can catalyze the high temperature decomposition stage of AP, which shows the superiority of the preparation method and also proves that the components of the RDX@Al / AP composite sample prepared by the Pickering emulsion method interact with each other, producing a synergistic effect to jointly improve the thermal properties of the composite.
[0116] The combustion performance of the physically mixed sample of Comparative Example 18 and the Zero-RDX@Al / AP prepared by the Pickering emulsion method of Comparative Example 1 was characterized by high-speed photography (Canon, EOSKiss70D). The results are as follows: Fig.12 As shown. The combustion process is carried out in an open system, using a Cr-Ni alloy wire with a diameter of 0.5mm and a melting point of about 1200℃ as the initial heating source, heated by a 7.5V DC power supply (MS-3010D, MAISHENG), igniting the sample, and recorded by high-speed photography (Canon, EOSKiss70D). The time from the first appearance of the spark represents the flame propagation process from the trigger signal, which is recorded as 0ms; until the spark disappears as a combustion process. Fig.12 (a) It can be seen that the total combustion time of the mixed sample prepared by the physical mixing method in Comparative Example 18 is 1473ms, and the most intense combustion moment is reached at 492ms. The flame color is golden yellow, the flame edge is blurred, and a large number of white solid particles are ejected. The uneven mixing between the components of the physical mixed sample and the large degree of dispersion between the particles are the main reasons for the difficulties in heat and mass transfer during the combustion process; this leads to the instability of the combustion process of the physical mixed sample and the long combustion time. In addition, during the combustion reaction, the thermal reaction of AP and RDX will produce gaseous products in a very short time, thereby causing the sputtering of Al powder. Therefore, in order to improve the combustion and energy release efficiency of the mixed sample and reduce the occurrence of sputtering, it is necessary to take corresponding measures to solve the problems of uneven sample mixing and particle dispersion. From Fig.12(b) It is found that the combustion time of the Zero-RDX@Al / AP composite sample is 540ms, and the most intense combustion moment is reached at about 180ms. The flame edge is smooth, the structure is clear, and it is a bright white flame. Compared with the physical mixed sample, the combustion time is shortened by 933ms, the reaction between the components is more thorough, and the overall flame temperature is relatively high. This is because the Zero-EM-RDX@Al / AP composite sample prepared by the Pickering emulsion method has a more uniform distribution of components, closer contact between components, and a shorter heat and mass transfer distance, which fully reflects the technical advantages of the Pickering emulsion method. At the same time, Example 1 and Example 2 use Al powder first coated with Fe2O3 and then modified with perfluorododecanoic acid as the core, and the combustion time of the prepared zero oxygen balance core-shell composite energetic material is 390ms and 398ms, indicating that the zero oxygen balance core-shell composite energetic material prepared by Example 1 and Example 2 has higher combustion performance and more concentrated energy release.
[0117] In order to explore the effect of Al content on the combustion performance of RDX@Al / AP composites, the combustion performance of the three core-shell composite samples of 1%-EM-RDX@Al / AP, 10%-EM-RDX@Al / AP, and 20%-EM-RDX@Al / AP in Comparative Examples 1 to 3 was tested. The results are shown in Figure 2. Fig.13 As shown, Fig.13 (a) is the combustion diagram of the 1%-EM-RDX@Al / AP sample, (b) is the combustion diagram of the 10%-EM-RDX@Al / AP sample, and (c) is the combustion diagram of the 20%-EM-RDX@Al / AP sample. When the content of modified Al powder is 1wt%, the combustion time is 974ms; the most intense combustion moment is reached at about 326ms, and the combustion is stable; when the proportion of modified Al powder is increased to 10wt%, the combustion time is 582ms; the most intense combustion moment is reached at about 194ms, and the combustion is stable; when the modified Al powder is further increased to 20wt%, the combustion time is only 218ms, and the deflagration phenomenon is found in a very short time after ignition. It can be seen that with the increase of Al content, the combustion process of RDX@Al / AP composite will be accelerated, and the time for the most intense combustion moment is shorter, and the combustion performance is significantly improved. Especially when the Al powder content reaches 20wt%, deflagration will occur. The main reason is that the redox reaction between the components causes rapid release of heat in a very short time, resulting in rapid gasification and decomposition of a large amount of RDX and AP and reaction, thus leading to the occurrence of deflagration.
[0118] Impact sensitivity and friction sensitivity are two important indicators for evaluating the safety of energetic materials, which are extremely important for the use, production and transportation of energetic materials. The test was conducted using the Chinese military standards GJB772A-97-601.2 (impact) and 602.1 (friction). The impact sensitivity test conditions are: drop weight: 10kg, charge: 50mg; a group of 25 samples are tested, and the drop weight height (H) at which the explosion probability is 50% is used. 50 ) represents the impact sensitivity, and the friction sensitivity test conditions are: swing angle: 90°, pressure: 3.92MPa, dosage: 20mg; 25 samples are tested in each group. The raw material RDX and 1%-EM-RDX@Al / AP prepared in comparative example 1 were tested for sensitivity. The results are shown in Fig.14 As shown. H of the raw material RDX 50 The friction sensitivity explosion percentage is 84%; the H 50 The impact sensitivity of the RDX@Al / AP composite is 24.29cm, and the explosion percentage of friction sensitivity is 96%. Compared with the raw material, the impact sensitivity of the RDX@Al / AP composite is increased by 9.8cm, which is mainly due to the advantages of the 1%-EM-RDX@Al / AP core-shell structure. When subjected to external impact, the relatively insensitive shell layer on the outside first absorbs part of the impact energy as a buffer, and then transfers the energy to the RDX in the inner core to form a hot spot and then trigger an explosion, so the impact sensitivity performance is significantly improved. However, compared with the friction sensitivity of the raw material, the explosion percentage of the friction sensitivity of 1%-EM-RDX@Al / AP is increased by 12%. From the SEM characterization results, the surface of the raw material RDX is smooth, and the surface of 1%-EM-RDX@Al / AP is rough, which will increase the friction coefficient between the particles when subjected to friction stress; secondly, the Al particles coated on the surface are hard in texture, and are prone to severe deformation with the RDX in the inner core when subjected to friction, resulting in an increase in friction sensitivity. According to the above method, the impact sensitivity and friction sensitivity of the zero oxygen balance core-shell composite energetic materials prepared in Example 1 and Example 2 were tested. The impact sensitivity H of the zero oxygen balance core-shell composite energetic materials prepared in Example 1 and Example 2 was 50 are 29.15 cm and 28.37 cm respectively, indicating that the impact sensitivity of the zero oxygen balance core-shell composite energetic materials prepared in Example 1 and Example 2 is further improved; at the same time, the friction sensitivity explosion percentages of the zero oxygen balance core-shell composite energetic materials prepared in Example 1 and Example 2 are 97% and 95% respectively, indicating that the coating of Al powder by Fe2O3 does not cause a significant decrease in the friction sensitivity of the zero oxygen balance core-shell composite energetic materials.
[0119] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.
[0120] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A modified aluminum powder, characterized in that: The aluminum powder is first coated with Fe2O3 to obtain the Fe2O3 coated aluminum powder, and then the Fe2O3 coated aluminum powder is modified with perfluorododecanoic acid.
2. A method for preparing the modified aluminum powder according to claim 1, characterized in that: The following steps are involved: S11, coating aluminum powder with Fe2O3 to obtain Fe2O3-coated aluminum powder; S12, dissolving perfluorododecanoic acid in ethyl acetate, and dispersing Fe2O3-coated aluminum powder in cyclohexane; S13. Under magnetic stirring, slowly drop ethyl acetate containing perfluorododecanoic acid into cyclohexane containing Fe2O3-coated aluminum powder, then continue stirring to react, filter, wash with cyclohexane several times, and put in an oven to dry for 2 to 6 hours to obtain modified aluminum powder.
3. The method for preparing modified aluminum powder according to claim 2, characterized in that: In the S11, the specific method of using Fe2O3 to coat aluminum powder includes: adding ammonia water to a ferric nitrate solution with a concentration of 0.1 to 0.5 mol / L, and stirring, and when a precipitate is generated, continuing to stir and adding aluminum powder and polyoxyethylene ether, ultrasonically oscillating at a frequency of 50 to 120 kHz for 10 to 20 minutes, standing and aging for 6 to 24 hours, and then separating the solid and liquid, washing the separated solid powder, vacuum freeze-drying, and then heating to 500 to 900°C at a heating rate of 2 to 4°C / min in an argon atmosphere, calcining for 1 to 3 hours, to obtain Fe2O3-coated aluminum powder; wherein the mass ratio of ferric nitrate to ammonia water is 1:1 to 2, and the mass ratio of the aluminum powder, ammonia water, and polyoxyethylene ether is 2 to 3:1:0.05 to 0.
2.
4. The method for preparing modified aluminum powder according to claim 2, characterized in that: In the S12, the mass volume ratio of perfluorododecanoic acid, ethyl acetate, aluminum powder and cyclohexane is 0.01 g:10-30 mL:1 g:100-300 mL.
5. The method for preparing modified aluminum powder according to claim 2, characterized in that: In S13, the magnetic stirring speed is 200-600 rpm; and the stirring reaction time is 1-3 h.
6. A method for preparing a zero oxygen balance core-shell composite energetic material containing modified aluminum powder, wherein the modified aluminum powder is prepared by the method for preparing the modified aluminum powder according to claims 2-3, characterized in that: include: adding cyclotrimethylene trinitramine into a solvent and dissolving it by ultrasonication to obtain a cyclotrimethylene trinitramine solution; Ammonium perchlorate is dissolved in water to obtain an ammonium perchlorate solution, and the ammonium perchlorate solution is added dropwise into a cyclotrimethylene trinitramine solution, ultrasonicated, and modified aluminum powder is added. The solution is ultrasonicated again, and the solution is allowed to stand and then vacuum freeze-dried to obtain a zero oxygen balance core-shell composite energetic material Zero-EM-RDX@Al / AP.
7. The method for preparing the zero oxygen balance core-shell composite energetic material containing modified aluminum powder according to claim 6, characterized in that: The solvent is ethyl acetate.
8. The method for preparing the zero oxygen balance core-shell composite energetic material containing modified aluminum powder according to claim 6, characterized in that: The mass volume ratio of cyclotrimethylene trinitramine, solvent, ammonium perchlorate, water and modified aluminum powder is 0.1-0.15 g: 2-6 mL: 0.05-0.1 g: 2-16 mL: 0.01-0.3 g.
9. The method for preparing the zero oxygen balance core-shell composite energetic material containing modified aluminum powder according to claim 6, characterized in that: The ultrasonic time after cyclotrimethylene trinitramine is added to the solvent is 4 to 10 minutes; The ultrasonic time after the ammonium perchlorate solution is added dropwise into the cyclotrimethylene trinitramine solution is 1 to 5 minutes; The ultrasonic time after adding the modified aluminum powder is 5 to 15 minutes, and the standing time is 0 to 40 minutes.
10. A zero oxygen balance core-shell composite energetic material containing modified aluminum powder, which is prepared by the preparation method of the zero oxygen balance core-shell composite energetic material containing modified aluminum powder according to any one of claims 6 to 9, characterized in that: include: The inner core is made of cyclotrimethylene trinitramine; The outer shell is coated on the outside of the inner core, and the outer shell is a composite material of modified aluminum powder and ammonium perchlorate.
Citation Information
Patent Citations
Micron-sized core-shell thermite and preparation method thereof
CN112341300A
RDX-Al composite energetic material and preparation method and application thereof
CN114835537A
(F + W) / O type emulsion and a cosmetic composition containing the same
JP6203322B1
Cited By
Aluminum powder perfluoropolyether polymer ammonium perchlorate composite energetic material and preparation method thereof
CN117843422A