Positive electrode material of lithium ion battery, preparation method of positive electrode material and positive plate
By using aromatic cores and acridinyl/acridine derivatives in the lithium-ion battery positive electrode material for coupling reaction, a lithium-ion battery positive electrode material with high energy density and excellent rate performance was prepared, solving the limited performance of the existing materials and environmentally friendly issues achieve more efficient battery performance and cycle life.
Patent Information
- Application Number
- CN202410921391.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-10
Smart Images

Figure CN118908893A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrode materials, and in particular to a lithium-ion battery positive electrode material and a preparation method thereof, and a positive electrode sheet. Background Art
[0002] Lithium-ion batteries, with their high energy density, long cycle life, and environmental friendliness, dominate the portable electronics market and show great promise in large-scale applications such as electric vehicles (EVs) and smart grids.
[0003] At present, lithium-ion batteries mainly use transition metal oxides or phosphates as positive electrodes, such as LiCoO2, LiMn2O4, LiFePO4 or LiNi x Mn y Co z O2, etc. They have high energy density, good conductivity and stable structure, and are widely used in life. Organic electrode materials have a wide range of sources, designable structures, are not restricted by ion types, and have the characteristics of sustainable resources and environmental friendliness.
[0004] However, inorganic electrode materials are often derived from non-renewable ores, while existing organic electrode materials have limited performance in terms of energy density, power density, and cycle life. Summary of the invention
[0005] In view of the deficiencies of the above-mentioned related technologies, the present application provides a lithium-ion battery positive electrode material and a preparation method thereof, and a positive electrode sheet.
[0006] In the first aspect, the present application provides a lithium-ion battery positive electrode material using the following technical solution: A lithium-ion battery positive electrode material, the structural formula of which is shown in the following formula I: , wherein R1 is an aromatic nucleus, at least two of R2, R3, R4 and R5 are acridinium groups / acridine derivative groups, and the rest are hydrogen atoms.
[0007] Preferably, at least two of R2, R3, R4 and R5 are the following groups: , the rest are hydrogen atoms; # indicates the connection position.
[0008] Preferably, the specific structural formula includes the following formulas (I-1) to (I-24): , , , , , , , , , , , , , , , , , , , , , , and Any of .
[0009] Preferably, its specific structural formula is , , and Any of .
[0010] In a second aspect, the present application provides a method for preparing a positive electrode material for a lithium-ion battery using the following technical solution: A method for preparing a positive electrode material for a lithium ion battery comprises the following steps: subjecting a halogenated aromatic compound and an acridine / acridine derivative to a coupling reaction to obtain the positive electrode material for the lithium ion battery.
[0011] Preferably, the method comprises the following steps: in an inert gas atmosphere, mixing acridine / acridine derivatives, halogenated aromatic compounds, solvents and additives for reaction for 10-14 hours, and purifying to obtain the lithium-ion battery positive electrode material.
[0012] Preferably, the additive includes one or more of palladium acetate, tri-tert-butylphosphine tetrafluoroborate, potassium tert-butoxide and potassium hydroxide.
[0013] Preferably, when the halogen atom in the halogenated aromatic compound is substituted on a benzene ring, the additive comprises palladium acetate, tri-tert-butylphosphine tetrafluoroborate and potassium tert-butoxide, and the molar ratio of the halogenated aromatic compound, palladium acetate, tri-tert-butylphosphine tetrafluoroborate and potassium tert-butoxide is 1:(0.03-0.09):(0.05-0.12):(4-8); the purification comprises the following steps: mixing the reacted substance with water, extracting with dichloromethane and concentrating the organic layer, and then purifying by silica gel column chromatography and then recrystallizing with dichloromethane and n-hexane.
[0014] Preferably, when the halogen atom in the halogenated aromatic compound is substituted on a benzene ring, the additive comprises palladium acetate, tri-tert-butylphosphine tetrafluoroborate and potassium tert-butoxide, and the molar ratio of the halogenated aromatic compound, palladium acetate, tri-tert-butylphosphine tetrafluoroborate and potassium tert-butoxide is 1:(0.03-0.09):(0.05-0.12):(4-8); the reaction temperature is 105-115°C; and the purification comprises the following steps: mixing the reacted substance with water, extracting with dichloromethane and concentrating the organic layer, and then purifying by silica gel column chromatography and then recrystallizing with dichloromethane and n-hexane.
[0015] Preferably, when the halogen atom in the halogenated aromatic compound is substituted on an alkyl group, the additive includes potassium hydroxide, and the molar ratio of the halogenated aromatic compound to the potassium hydroxide is 1:8-12; the purification includes the following steps: mixing the reacted substance with water, collecting the filter residue by vacuum filtration, and then purifying it through silica gel column chromatography and then recrystallizing it with n-hexane.
[0016] Preferably, when the halogen atom in the halogenated aromatic compound is substituted on an alkyl group, the additive includes potassium hydroxide, and the molar ratio of the halogenated aromatic compound to the potassium hydroxide is 1:8-12; the reaction temperature is room temperature; and the purification includes the following steps: mixing the reacted substance with water, collecting the filter residue by vacuum filtration, and then purifying it through silica gel column chromatography and then recrystallizing it with n-hexane.
[0017] Preferably, the eluent in the silica gel column chromatography purification process includes dichloromethane (DCM) and petroleum ether (PE).
[0018] Preferably, the volume ratio of dichloromethane (DCM) to petroleum ether (PE) is 1:3.5-4.5.
[0019] In the third aspect, the present application provides a positive electrode sheet adopting the following technical solution: A positive electrode sheet comprises the lithium ion battery positive electrode material, a conductive agent and a binder.
[0020] Preferably, the conductive agent includes one or more of conductive carbon black, graphene, carbon nanotubes, acetylene black, Ketjen black or ordered mesoporous carbon.
[0021] In a fourth aspect, the present application provides a lithium-ion battery adopting the following technical solution: A lithium ion battery comprises the positive electrode sheet, a separator, an electrolyte and a negative electrode sheet.
[0022] In summary, the present application includes at least one of the following beneficial technical effects: 1. With the aromatic core as the intermediate core, the acridinium group / acridine derivative group is located at the end of the intermediate core as an electropolymerization unit. On the one hand, the intermediate core determines the molecular aggregation state of the positive electrode material of the lithium-ion battery, and on the other hand, the acridinium group / acridine derivative group determines the molecular chemical structure of the positive electrode material of the lithium-ion battery. Under the joint action of the two, the reversible redox ability, electrochemical stability, rate performance, cycle performance and other battery performance of the positive electrode material of the lithium-ion battery as an organic electrode material are improved; 2. The lithium-ion battery cathode material of the present application exhibits a high discharge voltage exceeding 3.6 V, which improves the energy density of the battery; 3. When the nitrogen atoms in the positive electrode material of the lithium-ion battery of the present application are oxidized, they lose electrons to form positively charged cation radicals, which compensate for the charge by combining with large anions in the electrolyte, thereby improving the rate performance of the lithium-ion battery; 4. The electropolymerization behavior of the lithium-ion battery positive electrode material of the present application during the charge and discharge process is beneficial to improving the battery cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a comparison diagram of the aggregation structure of the lithium-ion battery positive electrode materials provided in Example 1 and Example 2 of the present application.
[0024] Figure 2 It is a comparison diagram of the aggregation structure of the lithium-ion battery positive electrode materials provided in Examples 3 and 4 of the present application.
[0025] Figure 3 This is a cycle performance diagram of the lithium-ion battery provided in Example 9 of the present application.
[0026] Figure 4 This is an infrared spectrum of the positive electrode sheet of Example 5 of the present application before and after the lithium-ion battery cycle test provided in Example 9.
[0027] Figure 5 This is a scanning electron microscope image of the positive electrode sheet of Example 5 of the present application before and after the lithium ion battery cycle test provided in Example 9.
[0028] Figure 6 It is a comparison chart of the rate performance of the lithium-ion batteries provided in Example 9 and Example 10.
[0029] Figure 7 It is a comparison chart of the rate performance of the lithium-ion batteries provided in Example 11 and Example 12.
[0030] Figure 8 This is a rate performance diagram of the lithium-ion battery provided in Example 9 under different activation current rate conditions.
[0031] Fig. 9It is a comparison diagram of the cyclic voltammetry curves of the lithium ion batteries provided in Examples 9-12.
[0032] Fig.10 It is a comparison diagram of constant current charge and discharge curves of the lithium ion batteries provided in Examples 9-12. DETAILED DESCRIPTION
[0033] The present application is further described in detail below in conjunction with examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. In the following examples, if specific conditions are not specified, they are carried out according to normal conditions or conditions recommended by the manufacturer. The methods used are conventional methods known in the art unless otherwise specified, and the consumables and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the recorded content may also be applied to the present invention. The raw materials used in the embodiments and comparative examples can be obtained commercially.
[0034] Example 1 Embodiment 1 of the present application provides a positive electrode material for a lithium ion battery, which is prepared by the following method: Under nitrogen atmosphere, 1, 4-dibromobenzene (400.0 mg, 1.71 mmol), 9,10-dihydro-9,9-dimethylacridine (715.8 mg, 3.42 mmol), palladium acetate (20.2 mg, 0.09 mmol), tri-tert-butylphosphine tetrafluoroborate (37.7 mg, 0.13 mmol) and potassium tert-butoxide (1151.3 mg, 10.26 mmol) were placed in a Schlenk reaction tube, toluene (20 mL) was added, and the mixture was heated to reflux at 110 °C for 12 h. After the reaction is completed, the mixture is cooled to room temperature, poured into water, extracted three times with dichloromethane, and the organic layer is concentrated to obtain a crude product. The crude product is purified by silica gel column chromatography (eluent: DCM: PE = 1:4), and recrystallized with dichloromethane and n-hexane to obtain a lithium ion battery positive electrode material as shown in formula (I-1) (white powder, 520 mg, yield: 62.1%).
[0035] The prepared lithium-ion battery positive electrode material having a structure as shown in formula (I-1) was characterized by nuclear magnetic resonance hydrogen spectrum, carbon spectrum and mass spectrum. The characterization data are as follows: 1 H NMR (400 MHz, CDCl3) δ (ppm): 7.61 (s, 4H,ArH), 7.50 (d, J = 7.3 Hz, 4H, ArH), 7.09 (t, J= 7.4 Hz, 4H, ArH), 6.99 (t, J =7.3 Hz, 4H, ArH), 6.45 (d, J = 8.0 Hz, 4H, ArH), 1.72 (s, 12H, -CH3). 13 C NMR (100 MHz, CDCl3) δ (ppm): 140.79, 133.95, 130.35, 126.50, 125.29, 120.90, 113.99, 36.06, 31.03. MS (EI, m / z ): [M] + Calculate for: C 36 H 32 N2, 492.67; Found:492.60.
[0036] Example 2 Embodiment 2 of the present application provides a positive electrode material for a lithium ion battery, which is prepared by the following method: Under nitrogen atmosphere, 2, 7-dibromofluorene (400.0 mg, 1.24 mmol), 9,10-dihydro-9,9-dimethylacridine (571.4 mg, 2.73 mmol), palladium acetate (13.5 mg, 0.06 mmol), tri-tert-butylphosphine tetrafluoroborate (26.1 mg, 0.09 mmol) and potassium tert-butoxide (834.8 mg, 7.44 mmol) were placed in a Schlenk reaction tube, toluene (20 mL) was added, and the mixture was heated to reflux at 110 °C for 12 h. After the reaction is completed, cool to room temperature, pour the reacted material into water, extract with dichloromethane three times, concentrate the organic layer to obtain a crude product, and purify the crude product by silica gel column chromatography (eluent: DCM: PE = 1:4), and recrystallize with dichloromethane and n-hexane to obtain a lithium ion battery positive electrode material as shown in formula (I-7) (light yellow powder, 350 mg, yield: 48.7%).
[0037] The prepared lithium-ion battery positive electrode material having a structure as shown in formula (I-7) was characterized by nuclear magnetic resonance hydrogen spectrum, carbon spectrum and mass spectrum. The characterization data are as follows: 1 H NMR (400 MHz, CDCl3) δ (ppm): 8.11 (d, J = 7.9Hz, 2H, ArH), 7.56 (s, 2H, ArH), 7.48 (d, J = 7.5 Hz, 4H, ArH), 7.42 (d, J= 7.9Hz, 2H, ArH), 7.01 – 6.90 (m, 8H, ArH), 6.37 (d, J = 7.6 Hz, 4H, ArH), 4.10 (s,2H, -CH2), 1.72 (s, 12H, -CH3). 13 C NMR (100 MHz, CDCl3) δ (ppm): 146.36,141.06, 140.93, 140.20, 130.25, 130.05, 128.11, 126.37, 125.31, 122.23,120.57, 114.10, 37.12, 36.02, 31.38. MS (EI, m / z ): [M] + Calculate for: C 43 H 36 N2,580.78; Found: 580.75.
[0038] Example 3 Embodiment 3 of the present application provides a positive electrode material for a lithium ion battery, which is prepared by the following method: Under nitrogen atmosphere, tri(4-bromophenyl)amine (400.0 mg, 0.84 mmol), 9,10-dihydro-9,9-dimethylacridine (544.2 mg, 2.60 mmol), palladium acetate (9.0 mg, 0.04 mmol), tri-tert-butylphosphine tetrafluoroborate (17.4 mg, 0.06 mmol) and potassium tert-butoxide (565.5 mg, 5.04 mmol) were placed in a Schlenk reaction tube, toluene (20 mL) was added, and the mixture was heated to reflux at 110 °C for 12 h. After the reaction is completed, cool to room temperature, pour the reacted material into water, extract with dichloromethane three times, concentrate the organic layer to obtain a crude product, and purify the crude product by silica gel column chromatography (eluent: DCM: PE = 1:4), and recrystallize with dichloromethane and n-hexane to obtain a lithium ion battery positive electrode material as shown in formula (I-17) (white powder, 450.0 mg, yield: 61.8%).
[0039] The prepared lithium-ion battery positive electrode material having a structure as shown in formula (I-17) was characterized by nuclear magnetic resonance hydrogen spectrum, carbon spectrum and mass spectrum. The characterization data are as follows: 1 H NMR (400 MHz, CDCl3) δ (ppm): 7.53 (d, J = 8.2Hz, 6H, ArH), 7.47 (d, J= 7.7 Hz, 6H, ArH), 7.34 (d, J = 8.2 Hz, 6H, ArH), 7.05(t, J = 7.6 Hz, 6H, ArH), 6.95 (t, J = 7.4 Hz, 6H, ArH), 6.46 (d, J = 8.1 Hz, 6H, ArH), 1.70 (s, 18H, -CH3). 13 C NMR (100 MHz, CDCl3) δ (ppm): 146.97, 141.07,136.19, 132.46, 130.20, 126.43, 126.28, 125.22, 120.66, 114.03, 36.01, 31.08. MS (MALDI-TOF) calcd. for C 63 H 54 N4[M+H] + : 866.43; Found: 866.60.
[0040] Example 4 Example 4 of the present application provides a positive electrode material for a lithium ion battery, which is prepared by the following method: 9,10-dihydro-9,9-dimethylacridine (753.4 mg, 3.60 mmol) and ground potassium hydroxide (504.9 mg, 9.00 mmol) were placed in a round-bottom flask, dissolved with N, N-dimethylformamide (20 mL), and stirred at room temperature for 1 h. Then, 1, 2, 4, 5-tetrabromomethylbenzene (400.0 mg, 0.90 mmol) was added in small amounts and batches, and stirred at room temperature for 12 h. At the end of the reaction, a precipitate was generated after adding water. After vacuum filtration, the filter residue was collected to obtain a crude product. After the crude product was separated and purified by silica gel chromatography, it was recrystallized using dichloromethane and n-hexane to obtain a lithium ion battery positive electrode material as shown in formula (I-22) (white powder, 150.0 mg, yield: 17.3%).
[0041] The prepared lithium-ion battery positive electrode material having a structure as shown in formula (I-22) was characterized by nuclear magnetic resonance hydrogen spectrum, carbon spectrum and mass spectrum. The characterization data are as follows: 1 H NMR (400 MHz, CDCl3) δ (ppm): 7.24 – 7.09 (m,8H, ArH), 6.79 (t, J= 7.4 Hz, 8H, ArH), 6.71 (d, J = 8.5 Hz, 10H, ArH), 6.39 (d, J = 7.6 Hz, 8H, ArH), 5.01 (s, 8H, -CH2), 1.34 (s, 24H, -CH3). 13 C NMR (100 MHz, CDCl3) δ (ppm): 139.84, 132.17, 131.57, 127.27, 126.19, 123.84, 120.42, 112.58, 47.50, 35.81, 28.96. MS (MALDI-TOF) calcd. for C 70 H 66 N4[M+H] + : 963.33;Found: 963.65.
[0042] Example 5 Embodiment 5 of the present application provides a positive electrode sheet, which is prepared by the following method: Weigh 40 mg of the positive electrode material for lithium-ion batteries prepared in Example 1 and 40 mg of conductive carbon black Super P in a mortar and grind them evenly. Add a mixed solution of polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP) at a mass ratio of 4:4:2 among the positive electrode material for lithium-ion batteries, conductive carbon black and polyvinylidene fluoride (PVDF). Transfer the mixed solution to a small beaker, stir and mix at 60 °C for 1 h, and then coat it on aluminum foil with a thickness of 120 μm. After vacuum drying at 100 °C for 12 h, slice it to obtain a 12 mm diameter and a loading of 0.9-1.2 mg cm -2 The positive electrode.
[0043] Example 6 Embodiment 6 of the present application provides a positive electrode sheet. Embodiment 6 differs from Embodiment 5 in that Embodiment 6 uses the lithium-ion battery positive electrode material prepared in Embodiment 2 to replace the lithium-ion battery positive electrode material prepared in Embodiment 1. Example 7 Embodiment 7 of the present application provides a positive electrode sheet. Embodiment 7 differs from Embodiment 5 in that Embodiment 7 uses the lithium-ion battery positive electrode material prepared in Embodiment 3 to replace the lithium-ion battery positive electrode material prepared in Embodiment 1.
[0044] Example 8 Embodiment 8 of the present application provides a positive electrode sheet. Embodiment 8 differs from Embodiment 5 in that Embodiment 8 uses the lithium-ion battery positive electrode material prepared in Embodiment 4 to replace the lithium-ion battery positive electrode material prepared in Embodiment 1.
[0045] Example 9 Embodiment 9 of the present application provides a lithium ion battery, which is prepared by the following method: First, place the negative electrode shell on the workbench, put the spring, gasket and negative electrode sheet (lithium sheet) in turn, drip 20 μL of electrolyte on the lithium sheet, place the diaphragm, drip 20 μL of electrolyte again, place the positive electrode sheet prepared in Example 5, cover the positive electrode shell, and use a battery packaging machine to pressurize and package the above components to obtain a lithium-ion battery (CR2032 button battery). After the battery is assembled, it needs to stand for more than 6 hours to ensure that the diaphragm and the positive electrode sheet can be fully infiltrated by the electrolyte. The electrolyte used is a solution of 1.0 M lithium hexafluorophosphate (LiPF6) dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) (v / v = 1 / 1).
[0046] Example 10 Embodiment 10 of the present application provides a lithium-ion battery. Embodiment 10 differs from Embodiment 9 in that Embodiment 10 uses the positive electrode sheet prepared in Embodiment 6 to replace the positive electrode sheet prepared in Embodiment 5.
[0047] Embodiment 11 Embodiment 11 of the present application provides a lithium-ion battery. Embodiment 11 differs from Embodiment 9 in that Embodiment 11 uses the positive electrode sheet prepared in Embodiment 7 to replace the positive electrode sheet prepared in Embodiment 5.
[0048] Example 12 Embodiment 12 of the present application provides a lithium-ion battery. Embodiment 12 differs from Embodiment 9 in that Embodiment 12 uses the positive electrode sheet prepared in Embodiment 8 to replace the positive electrode sheet prepared in Embodiment 5.
[0049] Test and Inspection (1) Detect the aggregation structure diagram of the lithium ion battery positive electrode material provided in Examples 1-4, such as Figure 1-2 As shown, Figure 1 (a) is a diagram showing the aggregate structure of the positive electrode material for a lithium-ion battery provided in Example 1; Figure 1 (b) is a diagram showing the aggregate structure of the positive electrode material for a lithium-ion battery provided in Example 2; Figure 2 (a) is a diagram showing the aggregate structure of the positive electrode material for a lithium-ion battery provided in Example 3; Figure 2 (b) is a diagram of the aggregation structure of the lithium-ion battery positive electrode material provided in Example 4.
[0050] (2) The cycle performance of the lithium ion battery provided in Example 9 was measured, and the cycle performance graph was obtained as shown in FIG. Figure 3 As shown, the positive electrode sheets in the lithium-ion battery before and after the cycle were detected and the infrared spectra were obtained as shown in Figure 4 As shown in the scanning electron microscope image Figure 5 shown.
[0051] (3) The rate performance of the lithium-ion batteries provided in Examples 9-12 was measured, and the rate performance graph was obtained as shown in FIG. Figure 6-8 As shown, Figure 6 The rate performance diagram of the lithium ion battery provided in Example 9 ( Figure 6 (a)) and the rate performance diagram of the lithium ion battery provided in Example 10 ( Figure 6 (b)) is a comparison chart, where Figure 7 The rate performance diagram of the lithium ion battery provided in Example 11 ( Figure 7 (a)) and the rate performance diagram of the lithium ion battery provided in Example 12 ( Figure 7 (b)) is a comparison chart, Figure 8 This is a rate performance diagram of the lithium-ion battery provided in Example 9 under different activation current rate conditions.
[0052] (4) Determine the cyclic voltammetry curves of the lithium ion batteries provided in Examples 9-12, such as Fig. 9 As shown, Fig. 9 (a) is a cyclic voltammetry curve of the lithium ion battery provided in Example 9; Fig. 9 (B) is a cyclic voltammetry curve of a lithium ion battery provided in Example 10; Fig. 9 (c) is a cyclic voltammetry curve of the lithium ion battery provided in Example 11; Fig. 9 (d) is a cyclic voltammetry curve of the lithium ion battery provided in Example 12.
[0053] (5) Determine the constant current charge and discharge curves of the lithium ion batteries provided in Examples 9-12, such as Fig.10 As shown, Fig.10 (a) is a constant current charge and discharge curve diagram of the lithium ion battery provided in Example 9; Fig.10 (b) is a constant current charge and discharge curve diagram of the lithium ion battery provided in Example 10; Fig.10 (c) is a constant current charge and discharge curve diagram of the lithium ion battery provided in Example 11; FIG. 12 (d) is a constant current charge and discharge curve diagram of the lithium ion battery provided in Example 12.
[0054] Results Analysis The following is a detailed description of this application in conjunction with the experimental data provided in Tables 1-10.
[0055] Reference Figure 1 and Figure 6 The lithium ion battery provided in Example 9 has a better rate performance than the lithium ion battery provided in Example 10, and the specific capacity of the lithium ion battery provided in Example 9 decreases less at 20C. Figure 1 It can be seen from the analysis that in the aggregation structure diagram of the lithium-ion battery positive electrode material used in the lithium-ion battery provided in Examples 9 and 10, the lithium-ion battery positive electrode material used in the lithium-ion battery provided in Example 9 has a closer polymerization site and a more planar polymerization mode than the lithium-ion battery positive electrode material used in the lithium-ion battery provided in Example 10, indicating that the intermediate core of the lithium-ion battery positive electrode material in Example 1 is beneficial to improve the rate performance of the prepared lithium-ion battery by changing the aggregation structure. And refer to Figure 8 The lithium-ion battery provided in Example 9 can still operate normally at a high rate of 100C, indicating that the material has excellent rate performance.
[0056] Reference Figure 2 and Figure 7 The rate performance of the lithium-ion battery provided in Example 11 is better than that of the lithium-ion battery provided in Example 12, and the rate performance of the lithium-ion batteries provided in Examples 11 and 12 is improved when the activation current rate is increased to 5C. Figure 2 From the analysis, it can be seen that in the aggregation structure diagram of the lithium ion battery positive electrode material used in the lithium ion battery provided in Example 11 and Example 12, the lithium ion battery positive electrode material used in the lithium ion battery provided in Example 11 has larger channels for ion transmission than the lithium ion battery positive electrode material used in the lithium ion battery provided in Example 12, indicating that the intermediate core of the lithium ion battery positive electrode material of Example 3 is beneficial to improving the rate performance of the prepared lithium ion battery by changing the aggregation structure.
[0057] Reference Figure 3 The lithium ion battery provided in Example 9 can still maintain 62.8 mAhg after 20,000 cycles at 50C. -1 The reversible capacity, capacity retention rate is 77.3%, the average capacity decay rate per cycle is 0.0011%, and the Coulomb efficiency is stable at 100%, showing excellent cycle performance. Figure 4 The infrared spectrum of the positive electrode sheet prepared in Example 5 shows that the positive electrode sheet after the cycle is at a wave number of 700-750 cm -1 The bending vibration peak of the ortho-disubstituted CH of the benzene ring disappears and is located at the wave number 800-820 cm -1 The 1, 2, 4-trisubstituted vibration peak of the benzene ring at 2400 nm appeared, proving that the acridine group underwent CC coupling polymerization during the battery cycle. Figure 5It can be seen from the scanning electron micrograph that the surface of the positive electrode sheet prepared in Example 5 is uniform and dense before the cycle, and particles of 100-300 nm in size appear on the surface after the cycle, indicating that as the cycle proceeds, a larger surface structure that is more conducive to electrode liquid infiltration and anion shuttling is formed on the surface of the positive electrode sheet prepared in Example 5, which is beneficial to improving the cycle performance of the lithium-ion battery.
[0058] Reference Fig. 9 As can be seen from the figure, the disappearance of the oxidation peak that appeared in the first forward scan indicated the occurrence of in-situ electropolymerization of the acridine group. The symmetry and reversibility of the scanning curve after the 5th cycle indicated that the polymerized material had excellent reversible redox ability and electrochemical stability.
[0059] Reference Fig.10 As can be seen from the figure, the lithium-ion batteries of Examples 9-12 all exhibit a discharge voltage of more than 3.6 V and a relatively high specific capacity, which is beneficial to the improvement of energy density; and as the cycle proceeds, the specific capacity and voltage of the lithium-ion battery positive electrodes of Examples 9, 10 and 12 gradually increase, showing a process of electropolymerization activation, indicating that the lithium-ion battery positive electrode material prepared by Examples 1-4 is beneficial to improving the discharge voltage, specific capacity and energy density of the lithium-ion battery.
Claims
1. A positive electrode material for a lithium-ion battery, characterized in that: Its structural formula is shown in the following formula I: , wherein R1 is an aromatic nucleus, at least two of R2, R3, R4 and R5 are acridinium groups / acridine derivative groups, and the rest are hydrogen atoms.
2. A lithium ion battery positive electrode material according to claim 1, characterized in that: At least two of R2, R3, R4 and R5 are the following groups: , the remainder are hydrogen atoms; # indicates the connection location.
3. A lithium ion battery positive electrode material according to claim 1, characterized in that: Its specific structural formula includes the following formulas (I-1) to (I-24): , , , , , , , , , , , , , , , , , , , , , , and Any of .
4. A method for preparing a positive electrode material for a lithium ion battery according to any one of claims 1 to 3, characterized in that: The following steps are involved: The halogenated aromatic compound and acridine / acridine derivative are subjected to coupling reaction to obtain the lithium ion battery positive electrode material.
5. The method for preparing a positive electrode material for a lithium ion battery according to claim 4, characterized in that: The following steps are involved: Under an inert gas atmosphere, acridine / acridine derivatives, halogenated aromatic compounds, solvents and additives are mixed and reacted for 10-14 hours, and purified to obtain the lithium-ion battery positive electrode material.
6. The method for preparing a positive electrode material for a lithium ion battery according to claim 5, characterized in that: The additive includes one or more of palladium acetate, tri-tert-butylphosphine tetrafluoroborate, potassium tert-butoxide and potassium hydroxide.
7. The method for preparing a positive electrode material for a lithium ion battery according to claim 6, characterized in that: When the halogen atom in the halogenated aromatic compound is substituted on a benzene ring, the additive comprises palladium acetate, tri-tert-butylphosphine tetrafluoroborate and potassium tert-butoxide, and the molar ratio of the halogenated aromatic compound, palladium acetate, tri-tert-butylphosphine tetrafluoroborate and potassium tert-butoxide is 1:(0.03-0.09):(0.05-0.12):(4-8); The purification comprises the following steps: mixing the reacted substance with water, extracting with dichloromethane and concentrating the organic layer, purifying with silica gel column chromatography and then recrystallizing with dichloromethane and n-hexane.
8. The method for preparing a positive electrode material for a lithium ion battery according to claim 6, characterized in that: When the halogen atom in the halogenated aromatic compound is substituted on an alkyl group, the additive includes potassium hydroxide, and the molar ratio of the halogenated aromatic compound to the potassium hydroxide is 1:8-12; The purification comprises the following steps: mixing the reacted substance with water, collecting the filter residue by vacuum filtration, purifying it by silica gel column chromatography, and then recrystallizing it with n-hexane.
9. A positive electrode sheet, characterized in that: The invention comprises the lithium ion battery positive electrode material according to any one of claims 1 to 3, a conductive agent and a binder.
10. A lithium ion battery, characterized in that: It comprises the positive electrode sheet, separator, electrolyte and negative electrode sheet as described in claim 9.
Citation Information
Patent Citations
Lithium ion secondary battery positive electrode materials of aromatic heterocyclic ketone compounds
CN103531810A
Lithium ion battery electrode material preparation method
CN106981661A
Organic compound, mixture, composition, electronic device and application
CN110746409A
Donor-acceptor type compound and application thereof in organic electroluminescence device
CN111574428A