Carboxylic butadiene-styrene latex for exterior wall coating and preparation method thereof
By using modified ultrafine silica and perfluoromethyl vinyl ether in exterior wall coatings, combined with PAMAM modified nanosilicon dioxide, the adhesion and stain resistance of carboxylic styrene butadiene latex are improved, and the solution is solved In the prior art, the problem of poor stain resistance of coatings has achieved better coating stability and service life.
Patent Information
- Application Number
- CN202410976490.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-20
- Publication Date
- 2024-11-08
AI Technical Summary
The existing exterior wall coatings have poor stain resistance and insufficient adhesion, which leads to powder falling off, dust accumulation, rainwater flow marks and powder fading in a short period of time after construction, which limits its widespread application.
Carboxy-butadiene latex, by using styrene and butadiene as main monomers, acrylic and itaconic acid as auxiliary monomers, combined with modified ultrafine silica and perfluoromethyl vinyl ether, pretreatment by acid , γ-aminopropyltriethoxysilane and PAMAM modified nanosilia to increase amino and silane groups, form chemical bonds and form dense protective films, improve adhesion and stain resistance.
It significantly improves the adhesion and stain resistance of exterior wall coatings, reduces the surface tension and water absorption of the coating film, forms tight adhesion, and extends the service life of the coating.
Smart Images

Figure BDA0004954698930000111
Abstract
Description
Technical Field
[0001] The present application relates to the field of preparation of styrene butadiene latex, and more specifically, to a carboxylated styrene butadiene latex for exterior wall coatings and a preparation method thereof. Background Art
[0002] In recent years, with the continuous development of high-rise buildings and the promotion and implementation of building energy conservation, lightweight wall materials have become the first choice for building exterior envelope systems. In order to improve the safety and durability of building exterior envelope systems and facilitate renovation and construction, exterior wall coatings have been vigorously promoted and widely used by the country as finishing materials. Exterior wall coatings are light in weight, have no safety hazards, and are beneficial to the earthquake resistance of buildings; they are available in a wide variety of varieties and rich colors to meet different design requirements; they are easy to renovate and can keep the building fresh.
[0003] Among exterior wall coatings, water-based exterior wall coatings are the main type of architectural coatings promoted due to people's emphasis on environmental protection. However, exterior wall latex coatings generally have problems such as poor stain resistance, coating powdering and shedding, and dust accumulation, rainwater runoff, coating powdering and fading gradually appear within 2-3 years after construction, limiting the promotion and application of exterior wall coatings. Therefore, for the emulsion used for exterior wall coatings, providing a new emulsion preparation to improve the adhesion of exterior wall coatings while improving stain resistance is of great significance for the wide application and performance improvement of exterior wall coatings. Summary of the invention
[0004] In order to prepare an emulsion that improves the adhesion of exterior wall paint and enhances the stain resistance, the present application provides a carboxylated styrene butadiene latex for exterior wall paint and a preparation method thereof.
[0005] In the first aspect, the present application provides a carboxylated styrene butadiene latex for exterior wall coatings, which adopts the following technical solution: A carboxylated styrene butadiene latex for exterior wall coating, comprising the following raw materials in parts by weight: 50-65 parts of styrene, 30-45 parts of butadiene, 5-12 parts of acrylate, 2-5 parts of acrylic acid, 3-5 parts of itaconic acid, 80-100 parts of water, 0.5-2.5 parts of emulsifier, 0.3-1.8 parts of initiator, 0.3-1 parts of pH buffer, 1-5 parts of seed latex, 0.01-0.05 parts of chelating agent, 1-3 parts of modified ultrafine silica and 0.1-0.5 parts of perfluoromethyl vinyl ether; The modified ultrafine silica is obtained by acid pretreatment of nano-silica and then sequentially modification with γ-aminopropyltriethoxysilane, PAMAM (polyamide-amine dendrimer) and benzaldehyde.
[0006] By adopting the above technical scheme, in this application, carboxylated styrene butadiene latex is prepared under the conditions of using styrene and butadiene as main monomers and carboxylic acid substances such as acrylic acid and itaconic acid as auxiliary monomers. For the improvement of the anti-fouling performance of carboxylated styrene butadiene latex for exterior wall coatings, lower surface tension and lower water absorption can significantly reduce the adsorption of dust and pollutants by the coating film, but the improvement of adhesion requires the addition of hydrophilic monomers and other measures, which is quite contradictory to the improvement of anti-fouling performance. Therefore, a small amount of modified ultrafine silica and perfluoromethyl vinyl ether are added in this application. The addition of modified ultrafine silica can quickly replenish the pores left after the volatilization of water due to its high free energy, thereby improving the flatness and anti-fouling performance of the coating film; The nano-silica is pretreated with acid to increase the number of hydroxyl groups on its surface, and then modified with γ-aminopropyltriethoxysilane to introduce amino and silane groups, and then modified with PAMAM, PAMAM is introduced to the surface of the nano-silica by grafting with amino groups, and then capped with benzaldehyde, which is more conducive to the uniformity of the dispersion of silica in the latex system. The branched structure of PAMAM gives it a larger specific surface area and more active sites, which improves the adhesion of carboxylated styrene butadiene latex while improving the density of the latex. PAMAM can form uniformly distributed nano-scale fillers in the latex, fill the tiny pores in the latex, enhance the density of the latex, and thus improve its stain resistance. It also plays the role of a surfactant to reduce the surface tension of the latex, which is more conducive to the formation of a close adhesion between the latex and the wall. Finally, the addition of modified ultrafine silica in this application significantly improves the stain resistance of the carboxylated styrene butadiene latex while improving its adhesion.
[0007] In addition, in the present application, when the nano-silica is modified with γ-aminopropyltriethoxysilane, a silane group is also introduced, so that the final carboxylated styrene butadiene latex can form a chemical bond with the surface group of the wall material, thereby improving the adhesion between the latex paint and the wall surface, and the silane group forms a dense protective film on the surface of the latex paint, improving the stain resistance of the latex paint. The introduction of fluorine element in perfluoromethyl vinyl ether further improves the stain resistance of the latex paint. Finally, the carboxylated styrene butadiene latex prepared in the present application has excellent adhesion and excellent stain resistance.
[0008] Optionally, the modified ultrafine silica is prepared by the following method: 1) Firstly, the nano-silicon dioxide is stirred in a nitric acid aqueous solution, and then acid-washed and modified at 55-70°C, and then washed with water after treatment for 40-60 minutes to obtain pre-treated silicon dioxide; 2) Add γ-aminopropyltriethoxysilane to anhydrous ethanol to obtain a mixed solution, then add the pretreated silica prepared in 1) to the mixed solution, stir at 60-80°C for 1.5-2.5h, then add PAMAM and genipin, react under ultrasonic-assisted conditions for 1-2h, finally add benzaldehyde, react for 20-30min, cool, filter, wash with water, and dry to obtain modified ultrafine silica.
[0009] By adopting the above technical scheme, nano silicon dioxide is first stirred in a nitric acid aqueous solution for acid washing modification to expose more hydroxyl groups on the surface, and then treated in a mixed solution containing γ-aminopropyltriethoxysilane. The γ-aminopropyltriethoxysilane reacts with the hydroxyl groups on the surface of silicon dioxide through condensation reaction and hydrolysis, thereby introducing amino groups on the surface of silicon dioxide. Then PAMAM is added to react with the amino groups on the surface of silicon dioxide, and then with the action of genipin, PAMAM and the amino groups on the surface of silicon dioxide are cross-linked, the cross-linking degree is increased, and the modification of silicon dioxide by PAMAM is achieved. Finally, benzaldehyde is added for end-capping reaction to obtain stable modified ultrafine silicon dioxide.
[0010] Optionally, during the preparation of modified ultrafine silica, the mass ratio of nano-silica and aqueous nitric acid solution is 1:(8-10), the amount of γ-aminopropyltriethoxysilane added is 8-10wt% of the nano-silica, the mixed liquid is 4-6 times the mass of the amount of pretreated silica added, the mass ratio of PAMAM to nano-silica is 1:(3-4), the amount of genipin added is 0.5-1wt% of the nano-silica, and the amount of benzaldehyde added is 3-5wt% of the nano-silica.
[0011] By adopting the above technical scheme, the ratio of the above raw materials is reasonably controlled, especially the control of the addition amount of PAMAM and nano-silica, so that the addition of a small amount of PAMAM can play the role of a stabilizer without demulsification and causing a decrease in the stability of the emulsion. Moreover, in the present application, PAMAM is modified and grafted on the nano-silica by γ-aminopropyltriethoxysilane and end-capped by benzaldehyde to avoid demulsification.
[0012] Optionally, the carboxylated styrene butadiene latex raw material further comprises 1-5 parts of modified polyurethane prepolymer, and the modified polyurethane prepolymer is prepared by modifying a polyurethane prepolymer solution with polyol, maleic anhydride and ethylenediamine.
[0013] Optionally, when preparing the modified polyurethane prepolymer, the polyol is selected from one or more of ethylene glycol, glycerol, diethylene glycol and pentaerythritol.
[0014] Optionally, the modified polyurethane prepolymer is prepared by the following method: In parts by weight, 3-8 parts of polyol are added to 20-30 parts of polyurethane prepolymer, and then 1-3 parts of emulsifier and 10-20 parts of water are added, and after mixing and stirring, 1-3 parts of maleic anhydride and 1-3 parts of ethylenediamine are added, and after stirring at 50-60° C. for 20-30 minutes, the modified polyurethane prepolymer is obtained after filtering.
[0015] By adopting the above technical scheme, a modified polyurethane prepolymer is also added in the preparation process of the carboxylated styrene butadiene latex of the present application, and the polyurethane prepolymer is modified by a polyol, and the polyol reacts with the isocyanate group in the prepolymer to form a waterborne polyurethane, and the polyol can also react with the NCO group in the prepolymer to form a three-dimensional network structure, and the addition of maleic anhydride and ethylenediamine can increase the chain length and crosslinking density of the polyurethane prepolymer. When preparing the carboxylated styrene butadiene latex in the present application, solution polymerization of the polyurethane prepolymer is carried out in a mixed monomer such as acrylate, and then the mixed monomer containing the polyurethane is emulsion polymerized to obtain an interpenetrating polymer network emulsion, which greatly improves the final anti-fouling performance of the carboxylated styrene butadiene latex.
[0016] Optionally, the polyurethane prepolymer is prepared by the following method: In parts by weight, 30-45 parts of polyoxypropylene glycol, 3-5 parts of dibutyltin dilaurate and 15-25 parts of butanone are mixed, the temperature is raised to 70-80° C., 80-90 parts of diphenylmethane diisocyanate are added under a nitrogen protective atmosphere, the mixture is kept warm for reaction for 1-2 hours, the temperature is lowered to 45-55° C., 8-15 parts of N-hydroxymethyldiethanolamine and 10-20 parts of 1,4-butanediol are added, the mixture is kept warm for reaction, and a polyurethane prepolymer is prepared.
[0017] By adopting the above technical solution, a small amount of modified polyurethane is added in the present application, which not only significantly improves the anti-fouling performance, but also reduces the amount of polyurethane used and reduces costs, which is conducive to large-scale promotion and application in construction.
[0018] Optionally, the emulsifier is selected from one or more of alkylphenol polyoxyethylene ether sulfate, alkyl diphenyl ether disulfonate, polyoxyethylene stearate, polysorbate and alkylphenol polyoxyethylene ether; The initiator is selected from one or more of potassium persulfate and ammonium persulfate; The chelating agent is disodium ethylenediaminetetraacetate.
[0019] By adopting the above technical scheme, alkylphenol polyoxyethylene ether sulfate and alkyl diphenyl ether disulfonate are used as anionic emulsifiers, polyoxyethylene stearate, polysorbate and alkylphenol polyoxyethylene ether are used as non-ionic emulsifiers. In the present application, the emulsifier is more preferably a mixture of the above two emulsifiers.
[0020] In a second aspect, the present application provides a method for preparing carboxylated styrene butadiene latex for exterior wall coatings, using the following technical solution: A method for preparing carboxylated styrene-butadiene latex for exterior wall coatings comprises the following steps: The styrene, butadiene, acrylate and perfluoromethyl vinyl ether are fully mixed and stirred to prepare an oil phase mixture; Mixing modified ultrafine silicon dioxide and 1 / 4 of the total added amount of water to prepare a first aqueous phase mixture; Mixing acrylic acid, a pH buffer, 1 / 4 of the total amount of water, and 2 / 3 of the total amount of emulsifier to prepare a second aqueous phase mixture; The initiator is mixed with 1 / 4 of the total amount of water to prepare an initiator mixture; The seed latex, disodium ethylenediaminetetraacetic acid, itaconic acid, the remaining water and the emulsifier are mixed and heated to 70-80° C. to prepare a primary mixture; The first aqueous phase mixture is added to the primary mixture to obtain a second mixture, and then the oil phase mixture, the second aqueous phase mixture and the initiator mixture are simultaneously added dropwise to the second mixture, reacting at 70-80°C for 5-6h, and then adjusting the pH, followed by degassing and cooling to obtain carboxylated styrene butadiene latex.
[0021] By adopting the above technical solution, in the present application, the oil phase mixture, the first water phase mixture, the second water phase mixture and the initiator mixture are prepared separately and then added dropwise for reaction, so that the polymerization reaction is more sufficient and uniform.
[0022] Optionally, the carboxylated styrene butadiene latex raw material further comprises 1-5 parts of modified polyurethane prepolymer; When preparing carboxylated styrene butadiene latex, modified polyurethane prepolymer and acrylate are added together.
[0023] By adopting the above technical solution, the modified polyurethane prepolymer and the acrylate monomer are added together, so that when the oil phase mixture is added to the second mixture for reaction, the modified polyurethane prepolymer is polymerized in the monomer solution, and polymerizes with acrylic acid, styrene and butadiene to obtain an interpenetrating polymer network emulsion, which greatly improves the final carboxylated styrene butadiene latex's stain resistance and adhesion.
[0024] In summary, this application has the following beneficial effects: 1. A small amount of modified ultrafine silica and perfluoromethyl vinyl ether are added in the present application. The introduction of fluorine in perfluoromethyl vinyl ether further improves the stain resistance of the latex coating. The addition of modified ultrafine silica can quickly replenish the pores left after the water evaporates due to its high free energy, thereby improving the flatness and stain resistance of the coating; 2. In the present application, the nano-silica is modified with γ-aminopropyltriethoxysilane to introduce amino and silane groups, and then modified with PAMAM, which is more conducive to the uniformity of the dispersion of silica in the latex system, and The branched structure of PAMAM gives it a larger specific surface area and more active sites, which improves the adhesion of carboxylated styrene butadiene latex while improving the compactness of the latex. Moreover, PAMAM can form uniformly distributed nano-scale fillers in the latex to fill the tiny pores in the latex, enhance the compactness of the latex, and thus improve its stain resistance. Moreover, it plays the role of a surfactant, reduces the surface tension of the latex, and is more conducive to the formation of a tight adhesion between the latex and the wall surface. Finally, the addition of modified ultrafine silica in this application significantly improves the stain resistance of the carboxylated styrene butadiene latex while improving its adhesion. 3. In the preparation process of the carboxylated styrene butadiene latex of the present application, a modified polyurethane prepolymer is also added, and the polyurethane prepolymer is modified by a polyol, and the polyol reacts with the isocyanate group in the prepolymer to form a water-based polyurethane, and the polyol can also react with the NCO group in the prepolymer to form a three-dimensional network structure, and the addition of maleic anhydride and ethylenediamine can increase the chain length and crosslinking density of the polyurethane prepolymer. When preparing the carboxylated styrene butadiene latex in the present application, solution polymerization of the polyurethane prepolymer is carried out in a mixed monomer such as acrylate, and then the mixed monomer containing the polyurethane is emulsion polymerized to obtain an interpenetrating polymer network emulsion, which greatly improves the final anti-fouling performance of the carboxylated styrene butadiene latex. DETAILED DESCRIPTION
[0025] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.
[0026] In the following examples, the alkylphenol polyoxyethylene ether ammonium sulfate emulsifier was selected from Nantong Huzhuo Chemical Co., Ltd. with specifications of CO436 and CAS of 9051-57-4; The seed latex in this application is prepared by the following method: 1.35 kg of deionized water and 0.05 kg of alkylphenol polyoxyethylene ether ammonium sulfate emulsifier are mixed, the temperature is raised to 60° C., and 0.05 kg of alkylphenol polyoxyethylene ether ammonium sulfate emulsifier and 1 kg of styrene monomer are added and mixed thoroughly to form a first material; 1.35 kg of water and 0.05 kg of alkylphenol polyoxyethylene ether ammonium sulfate emulsifier are mixed thoroughly to form a second material; The second material was uniformly added dropwise to the first material, and 0.03 kg of initiator (potassium persulfate and ammonium persulfate in a mass ratio of 1:1) was simultaneously added dropwise for 3 hours to obtain a seed latex.
[0027] Preparation Example 1 A method for preparing modified ultrafine silicon dioxide comprises the following steps: 1) Taking 1 kg of nano-silicon dioxide (particle size of 20-50 nm) as the treatment basis, the nano-silicon dioxide is first stirred in a nitric acid aqueous solution with a mass fraction of 27%, acid-washed and modified at 65° C., and then washed with water after treatment for 50 minutes to obtain pre-treated silicon dioxide; Among them, the added mass ratio of nano-silicon dioxide and nitric acid aqueous solution is 1:9; 2) Add γ-aminopropyltriethoxysilane to anhydrous ethanol to obtain a mixed solution, then add the pretreated silica prepared in 1) to the mixed solution, stir at 70° C. for 2 h, then add PAMAM and genipin, react under ultrasonic-assisted conditions for 1.5 h, finally add benzaldehyde, react for 25 min, cool, filter, wash with water, and dry to obtain modified ultrafine silica; Among them, in step 2), the addition amount of γ-aminopropyltriethoxysilane is 9wt% of the nano-silica, and the mixed liquid is 5 times the mass of the addition amount of pretreated silica, the mass ratio of PAMAM to nano-silica is 1:3.5, the addition amount of genipin is 0.7wt% of the nano-silica, and the addition amount of benzaldehyde is 4wt% of the nano-silica.
[0028] Preparation Example 2 A method for preparing modified ultrafine silicon dioxide comprises the following steps: 1) Taking 1 kg of nano-silicon dioxide (particle size of 20-50 nm) as the treatment basis, the nano-silicon dioxide is first stirred in a nitric acid aqueous solution with a mass fraction of 27%, acid-washed and modified at 55° C., and then washed with water after treatment for 60 minutes to obtain pre-treated silicon dioxide; Among them, the added mass ratio of nano-silicon dioxide and nitric acid aqueous solution is 1:8; 2) Add γ-aminopropyltriethoxysilane to anhydrous ethanol to obtain a mixed solution, then add the pretreated silica prepared in 1) to the mixed solution, stir at 60° C. for 2.5 h, then add PAMAM and genipin, react under ultrasonic-assisted conditions for 1 h, finally add benzaldehyde, react for 20 min, cool, filter, wash with water, and dry to obtain modified ultrafine silica; Wherein, in step 2), the amount of γ-aminopropyltriethoxysilane added is 8wt% of the nano-silica, and the mixed liquid is 4 times the mass of the amount of pretreated silica added, the mass ratio of PAMAM to nano-silica added is 1:3, the amount of genipin added is 0.5wt% of the nano-silica, and the amount of benzaldehyde added is 3wt% of the nano-silica.
[0029] Preparation Example 3 A method for preparing modified ultrafine silicon dioxide comprises the following steps: 1) Taking 1 kg of nano-silicon dioxide (particle size of 20-50 nm) as the treatment basis, the nano-silicon dioxide is first stirred in a nitric acid aqueous solution with a mass fraction of 27%, acid-washed and modified at 70° C., and then washed with water after treatment for 40 minutes to obtain pre-treated silicon dioxide; Among them, the added mass ratio of nano-silicon dioxide and nitric acid aqueous solution is 1:10; 2) Add γ-aminopropyltriethoxysilane to anhydrous ethanol to obtain a mixed solution, then add the pretreated silica prepared in 1) to the mixed solution, stir at 80° C. for 1.5 h, then add PAMAM and genipin, react under ultrasonic-assisted conditions for 2 h, finally add benzaldehyde, react for 30 min, cool, filter, wash with water, and dry to obtain modified ultrafine silica; Wherein, in step 2), the amount of γ-aminopropyltriethoxysilane added is 10wt% of the nano-silica, and the mixed liquid is 6 times the mass of the amount of pretreated silica added, the mass ratio of PAMAM to nano-silica added is 1:4, the amount of genipin added is 1wt% of the nano-silica, and the amount of benzaldehyde added is 5wt% of the nano-silica.
[0030] Comparative Preparation Example 1 A method for preparing modified ultrafine silicon dioxide comprises the following steps: 1) Firstly, the nano-silicon dioxide is stirred in a nitric acid aqueous solution, and then acid-washed and modified at 65°C, and then washed with water after treatment for 50 minutes to obtain pre-treated silicon dioxide; 2) Add γ-aminopropyltriethoxysilane to anhydrous ethanol to obtain a mixed solution, then add the pretreated silica prepared in 1) to the mixed solution, stir at 70° C. for 2 h, then cool, filter, wash with water and dry to obtain modified ultrafine silica.
[0031] Example 1 A method for preparing carboxylated styrene-butadiene latex for exterior wall coatings comprises the following steps: S1, 55 kg of styrene, 38 kg of butadiene, 10 kg of acrylate and 0.3 kg of perfluoromethyl vinyl ether were fully mixed and stirred to prepare an oil phase mixture; S2, 2 kg of the modified ultrafine silica prepared in Preparation Example 1 and 22.5 kg of water were mixed to prepare a first aqueous phase mixture; S3, 3 kg of acrylic acid, 0.5 kg of pH buffer (sodium hydroxide and sodium bicarbonate in a mass ratio of 1:1.5), 22.5 kg of water and 1 kg of emulsifier (a mixture of alkylphenol polyoxyethylene ether ammonium sulfate and Tween-80 in a mass ratio of 1:1) were mixed to prepare a second aqueous phase mixture; S4, mixing 1.2 kg of initiator (potassium persulfate and ammonium persulfate in a mass ratio of 1:1) and 22.5 kg of water to prepare an initiator mixture; S5, take 3kg seed latex and 0.03kg disodium ethylenediaminetetraacetic acid chelating agent, 4kg itaconic acid, 22.5kg water and 0.5kg emulsifier (mass ratio is 1: 1 mixture of alkylphenol polyoxyethylene ether ammonium sulfate and Tween-80), keep the vacuum degree at -0.075MPa, and heat to 75°C to obtain a primary mixture; S6. Add the first aqueous phase mixture to the primary mixture to obtain a second mixture, and then simultaneously drop the oil phase mixture, the second aqueous phase mixture and the initiator mixture into the second mixture for 3.5 hours. After the dropwise addition is completed, the mixture is kept warm for 2 hours at 75°C and a pressure of 0.4 MPa, and then a pH regulator, sodium bicarbonate, is added to adjust the pH to 7, and then degassing and cooling are performed to obtain carboxylated styrene butadiene latex.
[0032] Example 2 A method for preparing carboxylated styrene-butadiene latex for exterior wall coatings comprises the following steps: S1, 50 kg of styrene, 30 kg of butadiene, 5 kg of acrylate and 0.1 kg of perfluoromethyl vinyl ether were fully mixed and stirred to prepare an oil phase mixture; S2, mixing 1 kg of the modified ultrafine silicon dioxide prepared in Preparation Example 2 with 20 kg of water to prepare a first aqueous phase mixture; S3, mixing 2 kg of acrylic acid, 0.3 kg of pH buffer, 20 kg of water and 0.3 kg of emulsifier to prepare a second aqueous phase mixture; S4, mixing 0.3 kg of initiator and 20 kg of water to prepare an initiator mixture; S5, taking 1 kg of seed latex and mixing it with 0.01 kg of disodium ethylenediaminetetraacetic acid chelating agent, 3 kg of itaconic acid, 20 kg of water and 0.2 kg of emulsifier, maintaining the vacuum degree at -0.075 MPa, and heating to 70° C. to obtain a primary mixture; S6. Add the first aqueous phase mixture to the primary mixture to obtain a second mixture, and then simultaneously drop the oil phase mixture, the second aqueous phase mixture and the initiator mixture into the second mixture for 3 hours. After the dropwise addition, keep the mixture at 70°C and a pressure of 0.4 MPa for 2 hours, then add a pH adjuster, sodium bicarbonate, to adjust the pH to 7, and then degas and cool to obtain carboxylated styrene butadiene latex.
[0033] In this embodiment, the pH buffer is selected from sodium hydroxide and sodium bicarbonate in a mass ratio of 1:1.5, the emulsifier is selected from a mixture of alkylphenol polyoxyethylene ether ammonium sulfate and Tween-80 in a mass ratio of 1:1; and the initiator is selected from potassium persulfate and ammonium persulfate in a mass ratio of 1:1.
[0034] Example 3 A method for preparing carboxylated styrene-butadiene latex for exterior wall coatings comprises the following steps: S1. 65 kg of styrene, 45 kg of butadiene, 12 kg of acrylate and 0.5 kg of perfluoromethyl vinyl ether were fully mixed and stirred to prepare an oil phase mixture; S2, mixing 3 kg of the modified ultrafine silicon dioxide prepared in Preparation Example 3 and 25 kg of water to prepare a first aqueous phase mixture; S3, mixing 5 kg of acrylic acid, 1 kg of pH buffer, 25 kg of water and 1.7 kg of emulsifier to prepare a second aqueous phase mixture; S4, mixing 1.8 kg of initiator and 25 kg of water to prepare an initiator mixture; S5, taking 5kg of seed latex and mixing it with 0.05kg of disodium ethylenediaminetetraacetic acid chelating agent, 5kg of itaconic acid, 25kg of water and 0.8kg of emulsifier, maintaining the vacuum degree at -0.075MPa, and heating to 80°C to obtain a primary mixture; S6. Add the first aqueous phase mixture to the primary mixture to obtain a second mixture, and then simultaneously drop the oil phase mixture, the second aqueous phase mixture and the initiator mixture into the second mixture for 4 hours. After the dropwise addition, the mixture is kept warm for 2 hours at 80°C and a pressure of 0.4 MPa, and then a pH regulator, sodium bicarbonate, is added to adjust the pH to 8, and then degassing and cooling are performed to obtain carboxylated styrene butadiene latex.
[0035] In this embodiment, the pH buffer is selected from sodium hydroxide and sodium bicarbonate in a mass ratio of 1:1.5, the emulsifier is selected from a mixture of alkylphenol polyoxyethylene ether ammonium sulfate and Tween-80 in a mass ratio of 1:1; and the initiator is selected from potassium persulfate and ammonium persulfate in a mass ratio of 1:1.
[0036] Example 4 A method for preparing carboxylated styrene butadiene latex for exterior wall coating is carried out according to the method in Example 1, except that 3 kg of modified polyurethane prepolymer is added together with the acrylate in step S1, and the modified polyurethane prepolymer is prepared by the following method: a. In terms of weight, 38 kg of polyoxypropylene glycol, 4 kg of dibutyltin dilaurate and 20 kg of butanone were mixed, the temperature was raised to 75°C, 85 kg of liquefied MDI was added under a nitrogen atmosphere, the temperature was kept to react for 1.5 hours, the temperature was lowered to 50°C, and then 12 kg of N-hydroxymethyldiethanolamine and 15 kg of 1,4-butanediol were added, and the temperature was kept to react to obtain a polyurethane prepolymer; b. Take 28 kg of the polyurethane prepolymer prepared in step a, then add 5 kg of polyol, then add 2 kg of emulsifier and 15 kg of water, mix and stir, then add 2 kg of maleic anhydride and 2 kg of ethylenediamine, stir at 55 ° C for 25 minutes, and filter to obtain a modified polyurethane prepolymer.
[0037] Wherein, in step b, the polyol is a mixture of ethylene glycol and pentaerythritol in a mass ratio of 1:2, and the emulsifier is Tween 80.
[0038] Example 5 A method for preparing carboxylated styrene butadiene latex for exterior wall coating is carried out according to the method in Example 1, except that 1 kg of modified polyurethane prepolymer is added together with the acrylate in step S1, and the modified polyurethane prepolymer is prepared by the following method: a. In terms of weight, 30 kg of polyoxypropylene glycol, 3 kg of dibutyltin dilaurate and 15 kg of butanone were mixed, the temperature was raised to 70°C, 80 kg of liquefied MDI was added under a nitrogen atmosphere, the temperature was kept to react for 1 hour, the temperature was lowered to 45°C, and then 8 kg of N-hydroxymethyldiethanolamine and 10 kg of 1,4-butanediol were added, and the temperature was kept to react to obtain a polyurethane prepolymer; b. Take 20 kg of the polyurethane prepolymer prepared in step a, then add 3 kg of polyol, then add 1 kg of emulsifier and 10 kg of water, mix and stir, then add 1 kg of maleic anhydride and 1 kg of ethylenediamine, stir at 50 ° C for 30 minutes, and filter to obtain a modified polyurethane prepolymer.
[0039] Wherein, in step b, the polyol is a mixture of ethylene glycol and pentaerythritol in a mass ratio of 1:2, and the emulsifier is Tween 80.
[0040] Example 6 A method for preparing carboxylated styrene butadiene latex for exterior wall coating is carried out according to the method in Example 1, except that 5 kg of modified polyurethane prepolymer is added together with the acrylate in step S1, and the modified polyurethane prepolymer is prepared by the following method: a. In terms of weight, 45 kg of polyoxypropylene glycol, 5 kg of dibutyltin dilaurate and 25 kg of butanone were mixed, the temperature was raised to 80°C, 90 kg of liquefied MDI was added under a nitrogen atmosphere, the temperature was kept at room temperature for 2 hours, the temperature was lowered to 55°C, and 15 kg of N-hydroxymethyldiethanolamine and 20 kg of 1,4-butanediol were added, and the temperature was kept at room temperature for reaction to obtain a polyurethane prepolymer; b. Take 30 kg of the polyurethane prepolymer prepared in step a, then add 8 kg of polyol, then add 3 kg of emulsifier and 20 kg of water, mix and stir, then add 3 kg of maleic anhydride and 3 kg of ethylenediamine, stir at 60 ° C for 30 min, and filter to obtain a modified polyurethane prepolymer.
[0041] Wherein, in step b, the polyol is pentaerythritol and the emulsifier is Tween 80.
[0042] Example 7 A method for preparing carboxylated styrene butadiene latex in an exterior wall paint is carried out according to the method in Example 5, except that 3 kg of polyurethane prepolymer is added at the same time as the acrylate, and the polyurethane prepolymer is prepared by the method in Example 5 without being modified.
[0043] Comparative Example 1 A method for preparing carboxylated styrene butadiene latex in an exterior wall coating is carried out according to the method in Example 1, except that modified ultrafine silica is not added to the raw materials.
[0044] Comparative Example 2 A method for preparing carboxylated styrene butadiene latex in an exterior wall coating is carried out according to the method in Example 1, except that the modified ultrafine silica in step S2 is the modified ultrafine silica prepared in Comparative Preparation Example 1.
[0045] Comparative Example 3 A method for preparing carboxylated styrene butadiene latex for exterior wall coating is carried out according to the method in Example 1, except that in step S2, an equal amount of modified ultrafine silicon dioxide is replaced by unmodified nano silicon dioxide.
[0046] Comparative Example 4 A method for preparing carboxylated styrene butadiene latex for exterior wall coating is carried out according to the method in Example 1, except that no perfluoromethyl vinyl ether is added in step S1.
[0047] Comparative Example 5 A method for preparing carboxylated styrene butadiene latex for exterior wall coating is carried out according to the method in Example 1, except that an equal amount of perfluoromethyl vinyl ether in step S1 is replaced by polyvinylidene fluoride.
[0048] Performance Testing First, the carboxylated styrene butadiene latex products prepared in the examples and comparative examples of the present application were placed at 5° C., 25° C. and 40° C. for 12 months, respectively, without stratification, indicating that the prepared carboxylated styrene butadiene latex had good stability.
[0049] The carboxylated styrene butadiene latex prepared in the examples and comparative examples of the present application was used to prepare exterior wall coatings according to the following steps: First, 10kg of mica powder, 5kg of glass fiber, 12kg of kaolin and 10kg of titanium dioxide are premixed and added into 50kg of water for dispersion to obtain a primary mixture, and then 1.5kg of hydroxyethyl cellulose and 3kg of dispersant (HY-1030D water-resistant dispersant) are added and stirred, and then 0.5kg of defoamer (model DAPRO DF 7015) is added and stirred, and 20kg of carboxylated styrene butadiene latex is added, and finally 2kg of film-forming agent (a film-forming agent of model Coasol 290Plus and an alcohol ester twelve film-forming agent in a mass ratio of 1:2) and 0.5kg of preservative (BIT preservative and bactericide, specific model ELIMAVOB) are added, and the exterior wall coating is obtained after mixing and stirring.
[0050] The stain resistance of the exterior wall paint prepared above was tested with reference to GB / T 9755-2014, and its stain resistance was characterized by the reflection coefficient reduction rate (%). In addition, the adhesion of the exterior wall paint was tested according to ASTM D3359, and the adhesion was divided into 0-5 levels, 0 indicating no paint flakes falling off, and 5 indicating large-area paint flakes falling off. The test results are shown in Table 1 below.
[0051] Table 1: Referring to the test results in Table 1 above, the carboxylated styrene butadiene latex prepared in the embodiment of the present application has excellent stain resistance and excellent adhesion for exterior wall coatings. Combining the test results of Example 1 and Examples 4-6, it can be seen that when a modified polyurethane prepolymer is added to the raw material, the stain resistance is significantly improved and the adhesion is slightly improved. Combined with the test results in Example 7, the stain resistance of the raw material directly added with the polyurethane prepolymer without modification is slightly improved compared with Example 1, but it is lower than that of Example 4. For the addition of the modified polyurethane prepolymer, both the adhesion and stain resistance are improved; Referring to the test results of Example 1, Comparative Examples 1 and 3, when no modified ultrafine silica was added to Comparative Example 1, its anti-fouling performance and adhesion were significantly reduced. When unmodified ultrafine silica was added to Comparative Example 3, its anti-fouling performance was slightly improved compared with Comparative Example 1, and the adhesion was slightly different. Combined with the test results of Comparative Example 2, the nano-silica in Comparative Example 2 was modified by a silane coupling agent, and its anti-fouling performance was slightly improved, but it was far lower than the anti-fouling performance and adhesion performance in Example 1. Referring to the test results of Example 1, Comparative Examples 4 and 5, when no fluorinated ether substances were added to the raw materials, its anti-fouling performance and water resistance were reduced. Combined with the test results in Comparative Example 5, when only fluorine groups were introduced and no ether bond functional groups were contained, its anti-fouling performance was similar to that of Comparative Example 4, but the adhesion was reduced.
[0052] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A carboxylated styrene-butadiene latex for exterior wall coating, characterized in that: It includes the following raw materials in parts by weight: 50-65 parts of styrene, 30-45 parts of butadiene, 5-12 parts of acrylate, 2-5 parts of acrylic acid, 3-5 parts of itaconic acid, 80-100 parts of water, 0.5-2.5 parts of emulsifier, 0.3-1.8 parts of initiator, 0.3-1 parts of pH buffer, 1-5 parts of seed latex, 0.01-0.05 parts of chelating agent, 1-3 parts of modified ultrafine silica and 0.1-0.5 parts of perfluoromethyl vinyl ether; The modified ultrafine silica is obtained by acid pretreatment of nano-silica and then sequentially modification with γ-aminopropyltriethoxysilane, PAMAM and benzaldehyde.
2. The carboxylated styrene-butadiene latex for exterior wall coating according to claim 1, characterized in that: The modified ultrafine silica is prepared by the following method: 1) First, stir the nano-silicon dioxide in a nitric acid aqueous solution, perform acid washing modification at 55-70°C, treat for 40-60 minutes, and then wash with water to obtain pre-treated silicon dioxide; 2) Add γ-aminopropyltriethoxysilane to anhydrous ethanol to obtain a mixed solution, then add the pretreated silica prepared in 1) to the mixed solution, stir at 60-80°C for 1.5-2.5h, then add PAMAM and genipin, react under ultrasonic-assisted conditions for 1-2h, finally add benzaldehyde, react for 20-30min, cool, filter, wash with water and dry to obtain modified ultrafine silica.
3. The carboxylated styrene-butadiene latex for exterior wall coating according to claim 2, characterized in that: During the preparation process of modified ultrafine silica, the mass ratio of nano silica and nitric acid aqueous solution is 1: (8-10), the amount of γ-aminopropyltriethoxysilane added is 8-10wt% of the nano silica, the mixed liquid is 4-6 times the mass of the amount of pretreated silica added, the mass ratio of PAMAM to nano silica is 1: (3-4), the amount of genipin added is 0.5-1wt% of the nano silica, and the amount of benzaldehyde added is 3-5wt% of the nano silica.
4. The carboxylated styrene-butadiene latex for exterior wall coating according to claim 1, characterized in that: The carboxyl styrene butadiene latex raw material also includes 1-5 parts of modified polyurethane prepolymer, which is prepared by modifying a polyurethane prepolymer solution with polyol, maleic anhydride and ethylenediamine.
5. The carboxylated styrene-butadiene latex for exterior wall coating according to claim 4, characterized in that: When preparing the modified polyurethane prepolymer, the polyol is selected from one or more of ethylene glycol, glycerol, diethylene glycol and pentaerythritol.
6. The carboxylated styrene-butadiene latex for exterior wall coating according to claim 4, characterized in that: The modified polyurethane prepolymer is prepared by the following method: In parts by weight, 3-8 parts of polyol are added to 20-30 parts of polyurethane prepolymer, and then 1-3 parts of emulsifier and 10-20 parts of water are added, and after mixing and stirring, 1-3 parts of maleic anhydride and 1-3 parts of ethylenediamine are added, and after stirring at 50-60° C. for 20-30 minutes, the modified polyurethane prepolymer is obtained after filtering.
7. The carboxylated styrene-butadiene latex for exterior wall coating according to claim 4, characterized in that: The polyurethane prepolymer is prepared by the following method: In parts by weight, 30-45 parts of polyoxypropylene glycol, 3-5 parts of dibutyltin dilaurate and 15-25 parts of butanone are mixed, the temperature is raised to 70-80°C, 80-90 parts of diphenylmethane diisocyanate are added under a nitrogen protective atmosphere, the reaction is kept warm for 1-2 hours, the temperature is lowered to 45-55°C, and then 8-15 parts of N-hydroxymethyldiethanolamine and 10-20 parts of 1,4-butanediol are added, and the reaction is kept warm to obtain a polyurethane prepolymer.
8. The carboxylated styrene-butadiene latex for exterior wall coating according to claim 1, characterized in that: The emulsifier is selected from one or more of alkylphenol polyoxyethylene ether sulfate, alkyl diphenyl ether disulfonate, polyoxyethylene stearate, polysorbate and alkylphenol polyoxyethylene ether; The initiator is selected from one or more of potassium persulfate and ammonium persulfate; The chelating agent is disodium ethylenediaminetetraacetate.
9. A method for preparing a carboxylated styrene-butadiene latex for exterior wall coatings as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: The styrene, butadiene, acrylate and perfluoromethyl vinyl ether are fully mixed and stirred to prepare an oil phase mixture; Mixing modified ultrafine silicon dioxide and 1 / 4 of the total added amount of water to prepare a first aqueous phase mixture; Mixing acrylic acid, a pH buffer, 1 / 4 of the total amount of water, and 2 / 3 of the total amount of emulsifier to prepare a second aqueous phase mixture; The initiator is mixed with 1 / 4 of the total amount of water to prepare an initiator mixture; The seed latex, disodium ethylenediaminetetraacetic acid, itaconic acid, the remaining water and the emulsifier are mixed and heated to 70-80° C. to prepare a primary mixture; The first aqueous phase mixture is added to the primary mixture to obtain a second mixture, and then the oil phase mixture, the second aqueous phase mixture and the initiator mixture are simultaneously added dropwise to the second mixture, reacting at 70-80°C for 5-6h, and then adjusting the pH, followed by degassing and cooling to obtain carboxylated styrene butadiene latex.
10. The method for preparing carboxylated styrene-butadiene latex for exterior wall coating according to claim 9, characterized in that: The carboxyl styrene butadiene latex raw material also includes 1-5 parts of modified polyurethane prepolymer; When preparing carboxylated styrene butadiene latex, modified polyurethane prepolymer and acrylate are added together.