Vanadium electrolyte multifunctional polymer additive and preparation method thereof

The multifunctional polymer additive prepared by active radical polymerization solves the problem of poor stability of vanadium electrolyte at high concentrations by complexing carboxyl, amino and sulfonic acid groups with vanadium ions, widens the use temperature range, and improves the use temperature range The electrochemical performance and efficiency of vanadium batteries.

CN118909212AInactive Publication Date: 2024-11-08HANGZHOU DEHAI AIKE ENERGY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411419197.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing vanadium electrolytes are prone to supersaturation or supercritical states at high concentrations, resulting in poor stability. Commonly used additives will increase the density of the electrolyte and reduce the conductivity, making it difficult to effectively regulate the valence and electrochemical properties of vanadium.

Method used

Multifunctional polymer additives are prepared by active radical polymerization. Complex the carboxyl, amino and sulfonic acid groups with vanadium ions to form a protective layer or complex, inhibit vanadium ion agglomeration and particle agglomeration, and pass functional monomers and electrodes. Fiber association, improving electrochemical reversibility and kinetics.

Benefits of technology

The concentration stability of vanadium electrolyte is improved, the temperature range is widened, and the electrochemical performance is enhanced, especially under low and high temperature conditions, which improves the efficiency and stack performance of vanadium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909212A_ABST
    Figure CN118909212A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of vanadium redox flow battery electrolyte, in particular to a vanadium electrolyte multifunctional polymer additive and a preparation method thereof. The preparation method comprises the following steps: S1, weighing a specific amount of a reversible addition-fragmentation chain transfer reagent, a carboxyl or amino monomer, deionized water and an initiator, mixing and stirring, introducing nitrogen, and carrying out a heating reaction to obtain a mixed solution I; s2, weighing materials such as a sulfonic monomer, dissolving, adding the mixed solution I, and reacting to obtain a mixed solution II; s3, weighing materials such as functional monomers, adding the materials into the mixed solution II, and reacting to obtain a mixed solution III; and S4, filtering the mixed solution III, and performing vacuum drying and grinding to obtain the additive. The multifunctional polymer additive is added into a negative electrode electrolyte, additive functional groups are complexed with V < 2 + >, the concentration of the electrolyte is improved, and the low-temperature interval is widened; positive electrolyte is added to form a complex with VO < 2 + >, so that the effect of a dispersing agent is achieved, the concentration of the electrolyte is increased, and the high-temperature interval is widened; and the material can be adsorbed on the electrode surface to improve electrochemical performance and improve battery efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of vanadium liquid flow battery electrolyte, in particular to a multifunctional polymer additive for vanadium electrolyte and a preparation method thereof. Background Art

[0002] For commonly used vanadium electrolytes, the vanadium concentration is 1.5-1.8 mol / L. When the vanadium concentration is >1.5 mol / L, the acid concentration in the electrolyte needs to be precisely controlled at 3 mol / L, and the operating temperature is 10-40 °C. At this time, the operation of the electrolyte is basically in an oversaturated or supercritical state. In order to maintain the stable operation of high-concentration electrolytes, the research and development of stabilizers / additives has become a hot spot and focus of electrolyte research. When selecting additives, it is necessary to take into account the various valence states of V in the electrolyte and the impact on electrochemical properties. Commonly used additives are mainly inorganic salts, organic matter and polymers. Among them, the introduction of inorganic salts is equivalent to the introduction of impurity ions. Organic additives stabilize the valence state of vanadium by coordination and are usually used in large quantities, which easily increases the density of the electrolyte and leads to a decrease in conductivity. Active polymerization can precisely control the composition and segment order of the polymer, and can prepare block copolymers that cannot be achieved by traditional free radical polymerization. The polymer structure can be flexibly designed according to needs. Summary of the invention

[0003] The purpose of the present invention is to provide a multifunctional polymer additive for vanadium electrolyte and a preparation method thereof to solve the above problems.

[0004] The technical solution adopted by the present invention is as follows: A method for preparing a multifunctional polymer additive for vanadium electrolyte comprises the following steps: Step S1, weighing 3-9 parts by weight of a reversible addition-fragmentation chain transfer reagent, 10-30 parts by weight of a carboxyl or amino monomer, 100-150 parts by weight of deionized water and 0.2-0.6 parts of an initiator, mixing and stirring to dissolve, introducing nitrogen and heating to 70-85° C., reacting for 1.5-3 hours, to obtain a mixed solution 1; Step S2, weigh 5-30 parts by weight of sulfonic acid monomer, 40-80 parts by weight of deionized water and 0.2-0.6 parts by weight of initiator, mix and stir to dissolve, add to the mixed solution 1, heat to 75-90° C., react for 1.5-3 hours, and obtain the mixed solution 2; Step S3, weigh 0.5-1 parts by weight of functional monomer, 10-20 parts by weight of deionized water and 0.05-0.1 parts by weight of initiator, mix and stir to dissolve, then add to the mixed solution, heat to 75-90° C., react for 8-12 hours, and obtain a mixed solution III; Step S4, filtering the mixed solution, vacuum drying at 30-40° C. for 12-18 h and grinding with a mortar to obtain a multifunctional polymer additive.

[0005] Preferably, the reversible addition-fragmentation chain transfer reagent in step S1 is any one of 2-[(dodecylsulfanyl)thioacyl]-sulfanylpropionic acid, dithiophenylacetate pyridinium chloride, S-(2-propionic acid)-S'-(2-methylpropionic acid) trithiocarbonate, and dithiobenzoate pyridinium chloride.

[0006] Preferably, in step S1, the carboxyl or amino monomer is any one of acrylic acid, methacrylic acid, itaconic acid, acrylamide, methacrylamide, and hydroxymethyl acrylamide.

[0007] Preferably, the initiator in steps S1, S2 and S3 is any one of azobiscyanovaleric acid, ammonium persulfate, sodium persulfate and potassium persulfate.

[0008] Preferably, the sulfonic acid monomer in step S2 is any one of sodium methyl methacrylate sulfonate, sodium p-styrene sulfonate, and 2-acrylamido-2-methylpropane sulfonic acid.

[0009] Preferably, the functional monomer in step S3 is any one of tristyrylphenol polyethylene glycol methacrylate BOM25, alkoxy polyethylene glycol methacrylate BOM60, and double-bond-containing urea heterocyclic compound V-70M.

[0010] Preferably, the viscosity average molecular weight of the multifunctional polymer additive in step S4 is 1000-10000.

[0011] A multifunctional polymer additive for vanadium electrolyte is prepared by adopting the preparation method of the multifunctional polymer additive for vanadium electrolyte.

[0012] The beneficial effects of the present invention are: 1. The multifunctional polymer additive of the present invention is added to the negative electrode electrolyte, and the carboxyl group, amino group and sulfonic acid group on the polymer additive can react with V 2+ The complexation with the functional group increases the outer charge and generates electrostatic repulsion, forming a protective layer that hinders V 2+ Agglomeration forms precipitation, which increases the concentration of vanadium electrolyte and broadens the low-temperature range of vanadium electrolyte use.

[0013] 2. The multifunctional polymer additive of the present invention is added to the positive electrode electrolyte. On the one hand, the carboxyl group, amino group and sulfonic acid group on the polymer additive can react with VO2 + The additive forms a complex, inhibits the nucleation and crystallization of V2O5, and reduces the attraction between particles to reduce particle aggregation. On the other hand, the additive plays the role of a dispersant. Based on the combined effects of Coulomb repulsion and steric hindrance, it can promote the dispersion of hydrated pentavalent vanadium ions, thereby increasing the concentration of vanadium electrolyte and broadening the high-temperature range of vanadium electrolyte use.

[0014] 3. The multifunctional polymer additive of the present invention can be adsorbed on the electrode surface through the association of functional monomers with electrode fibers, thereby improving the electrochemical reversibility and kinetics of the redox couple on the electrode and improving the efficiency of the vanadium battery.

[0015] 4. The multifunctional polymer additive of the present invention adopts the method of active free radical polymerization. The polymer chain segment contains a block structure of multiple functional groups. The ratio between the functional groups can be adjusted at will, and the role of each functional group can be fully exerted. Adding it to the vanadium electrolyte can reduce the dosage. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a synthesis mechanism diagram of the polymer additive acrylic acid / sodium p-phenylene sulfonate of Example 1 of the present invention; Figure 2 This is the infrared spectrum of the multifunctional polymer additive acrylic acid / sodium p-phenylene sulfonate in Example 1 of the present invention. DETAILED DESCRIPTION

[0017] The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] A method for preparing a multifunctional polymer additive for vanadium electrolyte comprises the following steps: Step S1, weighing 3-9 parts by mass of a reversible addition-fragmentation chain transfer reagent, 10-30 parts by mass of a carboxyl or amino monomer, 100-150 parts by mass of deionized water and 0.2-0.6 parts by mass of an initiator, mixing and stirring to dissolve, introducing nitrogen and heating to 70-85° C., reacting for 1.5-3 hours, to obtain a mixed solution 1; wherein the reversible addition-fragmentation chain transfer reagent is any one of 2-[(dodecylsulfanyl)thioacyl]-sulfanylpropionic acid, dithiophenylacetic acid ester pyridinium chloride, S-(2-propionic acid)-S'-(2-methylpropionic acid) trithiocarbonate, and dithiobenzoate pyridinium chloride; the carboxyl or amino monomer is any one of acrylic acid, methacrylic acid, itaconic acid, acrylamide, methacrylamide, and hydroxymethyl acrylamide; the initiator is any one of azobiscyanovaleric acid, ammonium persulfate, sodium persulfate, and potassium persulfate; Step S2, weighing 5-30 parts by weight of sulfonic acid monomer, 40-80 parts by weight of deionized water and 0.2-0.6 parts by weight of initiator, mixing and stirring to dissolve, and then adding to the mixed solution 1, heating to 75-90° C., reacting for 1.5-3 hours, to obtain a mixed solution 2; the sulfonic acid monomer is any one of sodium methyl propylene sulfonate, sodium p-styrene sulfonate, and 2-acrylamido-2-methylpropane sulfonic acid; the initiator is any one of azobiscyanovaleric acid, ammonium persulfate, sodium persulfate, and potassium persulfate; Step S3, weighing 0.5-1 parts by weight of functional monomer, 10-20 parts by weight of deionized water and 0.05-0.1 parts by weight of initiator, mixing and stirring to dissolve, adding the mixture to the mixed solution, heating to 75-90° C., reacting for 8-12 hours, and obtaining a mixed solution three; wherein the functional monomer is any one of tristyrylphenol polyethylene glycol methacrylate BOM25, alkoxy polyethylene glycol methacrylate BOM60, and double-bond-containing urea heterocyclic compound V-70M; and the initiator is any one of azobiscyanovaleric acid, ammonium persulfate, sodium persulfate, and potassium persulfate; Step S4, filtering the mixed solution, vacuum drying at 30-40° C. for 12-18 hours and grinding with a mortar to obtain a multifunctional polymer additive; wherein the viscosity average molecular weight of the multifunctional polymer additive is 1000-20000.

[0019] Example 1

[0020] A method for preparing a multifunctional polymer additive for vanadium electrolyte comprises the following steps: Step S1, weighing 5 parts by mass of a reversible addition-fragmentation chain transfer reagent 2-[(dodecylsulfanyl)thioacyl]-sulfanylpropionic acid, 15 parts by mass of an acrylic acid monomer, 120 parts by mass of deionized water and 0.3 parts by mass of an initiator azobiscyanovaleric acid, mixing and stirring to dissolve, introducing nitrogen and heating to 75° C., reacting for 2 hours, to obtain a mixed solution 1; Step S2, weighing 15 parts by mass of sodium styrene sulfonate monomer, 60 parts by mass of deionized water and 0.3 parts by mass of initiator azobiscyanovaleric acid, stirring and mixing to dissolve, and then adding to the mixed solution 1, heating to 80° C., reacting for 10 hours, to obtain a mixed solution 2; Step S3, weighing 0.5-1 parts by weight of functional monomer tristyrylphenol polyethylene glycol methacrylate BOM25, 15 parts by weight of deionized water and 0.08 parts by weight of initiator azobiscyanovaleric acid, stirring and mixing to dissolve, adding the mixture to the mixed solution, heating to 85° C., reacting for 10 hours, to obtain a mixed solution three; Step S4, filtering the mixed solution, vacuum drying at 35°C for 16 hours and grinding with a mortar to obtain a multifunctional polymer additive; wherein the viscosity average molecular weight of the multifunctional polymer additive is 4000; Depend on Figure 1 As shown, in this embodiment, a multifunctional polymer additive is synthesized by three reactions of living free radical polymerization, and the polymer chain segments contain multiple functional groups. Figure 2 It can be seen that at 1008, 1037, 1190cm -1 There is a strong absorption peak of sulfonic acid group at 3030cm -1 The stretching vibration absorption peak of benzene ring CH is 835cm -1 The presence of disubstituted benzene rings in the structure is indicated at 675 cm -1 Out-of-plane stretching vibration peak of -CH substituted benzene ring structure, 1450~1650cm -1 The peak of the skeleton vibration of the benzene ring is 2922 cm -1 The absorption peak of -CH2 is 3450cm -1 is the stretching vibration peak of the associated -OH, 1120 cm -1 is the absorption peak of CO bond, 1725cm -1 It is the absorption peak of C=O in the carboxyl group, and there is no absorption peak of unsaturated double bond in the spectrum, indicating that the multifunctional polymer additive has been successfully prepared.

[0021] Example 2

[0022] A method for preparing a multifunctional polymer additive for vanadium electrolyte comprises the following steps: Step S1, weighing 6 parts by mass of a reversible addition-fragmentation chain transfer reagent dithiophenylacetate pyridinium chloride, 18 parts by mass of a methacrylic acid monomer, 100 parts by mass of deionized water and 0.4 parts by mass of an initiator sodium persulfate, mixing and stirring to dissolve, introducing nitrogen and heating to 80° C., reacting for 2 hours, to obtain a mixed solution 1; Step S2, weighing 20 parts by mass of sodium styrene sulfonate monomer, 40 parts by mass of deionized water and 0.4 parts by mass of initiator sodium persulfate, mixing and stirring to dissolve, and then adding to the mixed solution 1, heating to 85° C., reacting for 2 hours, to obtain a mixed solution 2; Step S3, weighing 0.5 parts by mass of functional monomer alkoxy polyethylene glycol methacrylate BOM60, 10 parts by mass of deionized water and 0.05 parts by mass of initiator sodium persulfate, mixing and stirring to dissolve, and then adding to the mixed solution, heating to 75° C., reacting for 11 hours, to obtain a mixed solution three; Step S4, filtering the mixed solution, vacuum drying at 30° C. for 12 h and grinding with a mortar to obtain a multifunctional polymer additive; wherein the viscosity average molecular weight of the multifunctional polymer additive is 6000.

[0023] Example 3

[0024] A method for preparing a multifunctional polymer additive for vanadium electrolyte comprises the following steps: Step S1, weighing 3 parts by mass of a reversible addition-fragmentation chain transfer reagent 2-[(dodecylsulfanyl)thioacyl]-sulfanylpropionic acid, 30 parts by mass of itaconic acid monomer, 150 parts by mass of deionized water and 0.2 parts by mass of an initiator ammonium persulfate, mixing and stirring to dissolve, introducing nitrogen and heating to 85° C., reacting for 3 hours, to obtain a mixed solution 1; Step S2, weighing 30 parts by mass of sodium methyl propylene sulfonate monomer, 80 parts by mass of deionized water and 0.2 parts by mass of initiator ammonium persulfate, mixing and stirring to dissolve, and then adding to the mixed solution 1, heating to 90° C., reacting for 3 hours, to obtain the mixed solution 2; Step S3, weighing 1 part by mass of a functional monomer containing a double bond urea heterocyclic compound V-70M, 20 parts by mass of deionized water and 0.1 parts by mass of an initiator ammonium persulfate, mixing and stirring to dissolve, and then adding the mixture to the mixed solution, heating to 90° C., reacting for 8 hours, to obtain a mixed solution III; Step S4, filtering the mixed solution, vacuum drying at 40° C. for 18 h and grinding with a mortar to obtain a multifunctional polymer additive; wherein the viscosity average molecular weight of the multifunctional polymer additive is 10,000.

[0025] Example 4

[0026] A method for preparing a multifunctional polymer additive for vanadium electrolyte comprises the following steps: Step S1, weighing 7 parts by mass of a reversible addition-fragmentation chain transfer reagent S-(2-propionic acid)-S'-(2-methylpropionic acid) trithiocarbonate, 25 parts by mass of acrylamide monomer, 130 parts by mass of deionized water and 0.3 parts by mass of an initiator potassium persulfate, mixing and stirring to dissolve, introducing nitrogen and heating to 70° C., reacting for 3 hours, to obtain a mixed solution 1; Step S2, weigh 10 parts by mass of sodium methyl propylene sulfonate monomer, 50 parts by mass of deionized water and 0.3 parts by mass of initiator potassium persulfate, mix and stir to dissolve, then add to the mixed solution 1, heat to 75° C., react for 3 hours, and obtain the mixed solution 2; Step S3, weighing 0.7 parts by mass of functional monomer tristyrylphenol polyethylene glycol methacrylate BOM25, 15 parts by mass of deionized water and 0.08 parts by mass of initiator potassium persulfate, mixing and stirring to dissolve, and then adding to the mixed solution, heating to 80° C., reacting for 12 hours, to obtain a mixed solution three; Step S4, filtering the mixed solution, vacuum drying at 40° C. for 14 h and grinding with a mortar to obtain a multifunctional polymer additive; wherein the viscosity average molecular weight of the multifunctional polymer additive is 3500.

[0027] Example 5

[0028] A method for preparing a multifunctional polymer additive for vanadium electrolyte comprises the following steps: Step S1, weighing 9 parts by mass of a reversible addition-fragmentation chain transfer reagent dithiobenzoate pyridinium chloride, 10 parts by mass of acrylamide monomer, 140 parts by mass of deionized water and 0.6 parts by mass of initiator ammonium persulfate, mixing and stirring to dissolve, introducing nitrogen and heating to 85° C., reacting for 1.5 hours, to obtain a mixed solution 1; Step S2, weighing 5 parts by mass of 2-acrylamide-2-methylpropanesulfonic acid monomer, 70 parts by mass of deionized water and 0.6 parts by mass of initiator ammonium persulfate, mixing and stirring to dissolve, and then adding to the mixed solution 1, heating to 90° C., reacting for 1.5 hours, to obtain the mixed solution 2; Step S3, weighing 0.8 parts by mass of functional monomer tristyrylphenol polyethylene glycol methacrylate BOM25, 10 parts by mass of deionized water and 0.07 parts by mass of initiator ammonium persulfate, mixing and stirring to dissolve, and then adding to the mixed solution, heating to 85° C., reacting for 9 hours, to obtain a mixed solution three; Step S4, filtering the mixed solution, vacuum drying at 30° C. for 15 h and grinding with a mortar to obtain a multifunctional polymer additive; wherein the viscosity average molecular weight of the multifunctional polymer additive is 1000.

[0029] Example 6

[0030] A method for preparing a multifunctional polymer additive for vanadium electrolyte comprises the following steps: Step S1, weighing 8 parts by mass of a reversible addition-fragmentation chain transfer reagent 2-[(dodecylsulfanyl)thioacyl]-sulfanylpropionic acid, 20 parts by mass of acrylamide monomer, 120 parts by mass of deionized water and 0.3 parts by mass of an initiator azobiscyanovaleric acid, mixing and stirring to dissolve, introducing nitrogen and heating to 80° C., reacting for 2 hours, to obtain a mixed solution 1; Step S2, weighing 25 parts by mass of sodium p-styrene sulfonate monomer, 60 parts by mass of deionized water and 0.3 parts by mass of initiator azobiscyanovaleric acid, mixing and stirring to dissolve, and then adding to the mixed solution 1, heating to 85° C., reacting for 2 hours, to obtain a mixed solution 2; Step S3, weighing 0.6 parts by mass of functional monomer alkoxy polyethylene glycol methacrylate BOM60, 20 parts by mass of deionized water and 0.06 parts by mass of initiator azobiscyanovaleric acid, stirring and mixing to dissolve, and then adding to the mixed solution, heating to 80° C., reacting for 11 hours, to obtain a mixed solution three; Step S4, filtering the mixed solution, vacuum drying at 35° C. for 14 h and grinding with a mortar to obtain a multifunctional polymer additive; wherein the viscosity-average molecular weight of the multifunctional polymer additive is 8000.

[0031] Comparative Example 1 Consistent with Example 1, free radical copolymerization was carried out without using a chain transfer agent.

[0032] Comparative Example 2 Consistent with Example 1, step S3 is not performed.

[0033] Comparative Example 3 Commonly used polymer additive polyacrylic acid.

[0034] Comparative Example 4 No additives.

[0035] Using electrolysis to produce 2.5 mol / L VO2 + Positive vanadium electrolyte, and 2.5 mol / L V 2+ The negative electrode vanadium electrolyte is prepared by adding the additives of the embodiment and the comparative example to VO2 + Cathode vanadium electrolyte and V 2+ The amount of the added negative electrode vanadium electrolyte was 0.4% of the total mass of the vanadium electrolyte, and the electrolyte was placed at -20°C, 25°C and 60°C respectively. The sedimentation of the vanadium electrolyte was observed after 72 hours. The results are shown in the following table: Table 1 Additives used in Examples and Comparative Examples to VO2 + and V 2+ Stability in vanadium electrolyte

[0036] The polymer additives of the vanadium electrolyte of the embodiment and the comparative example were added to the vanadium electrolyte, and the addition amount was 0.4% of the total mass of the vanadium electrolyte, and the stack was assembled for testing. The coulombic efficiency, voltage efficiency and energy efficiency were tested and recorded under the same test conditions. The test results are shown in the following table: Table 2: Test table of stack performance using additives from examples and comparative examples added to vanadium electrolyte

[0037] As shown in Table 1, the multifunctional polymer additive of the embodiment is added to 2.5 mol / L VO2 + The positive electrode vanadium electrolyte has good stability, and the electrolyte has no precipitation at 60°C for 72 hours, which shows that the multifunctional polymer additive of the present invention is added to the positive electrode electrolyte. On the one hand, the carboxyl group, amino group and sulfonic acid group on the polymer additive can react with VO2 + The additive forms a complex, inhibits the nucleation and crystallization of V2O5, and reduces the attraction between particles to reduce particle aggregation. On the other hand, the additive plays the role of a dispersant. Based on the combined effect of Coulomb repulsion and steric hindrance, it can promote the dispersion of hydrated pentavalent vanadium ions, thereby increasing the concentration of vanadium electrolyte and broadening the high temperature range of vanadium electrolyte. 2+The stability of the negative electrode vanadium electrolyte is good, indicating that the carboxyl group, amino group and sulfonic acid group on the multifunctional polymer additive of the present invention can react with V 2+ Functional groups are complexed, and the outer layer charge increases to generate electrostatic repulsion, forming a protective layer that hinders V 2+ Agglomeration forms a precipitate, which increases the concentration of the vanadium electrolyte and broadens the low-temperature range of the vanadium electrolyte. The polymer additive prepared in Comparative Example 1 has a worse stabilizing effect on the vanadium electrolyte than Example 1, but is better than the blank resistor in Comparative Example 4. This is because the multifunctional polymer additive of the present invention adopts the method of active free radical polymerization, and the polymer chain segment contains a block structure of multiple functional groups. The ratio between the functional groups can be adjusted at will, and the role of each functional group can be fully exerted. Adding it to the vanadium electrolyte can reduce the dosage. Compared with Example 1, Comparative Example 2 has a poorer stabilizing effect on the vanadium electrolyte, indicating that the functional monomers in the polymer additive do not affect the stability of the vanadium electrolyte. The commonly used polymer additives in Comparative Example 3 have a worse stabilizing effect on the vanadium electrolyte than Example 1, but are better than the blank resistor in Comparative Example 4, indicating that commonly used polymer additives can stabilize the vanadium electrolyte, but the effect is relatively limited.

[0038] As can be seen from Table 2, the embodiments all have high voltage efficiency and energy efficiency. This is because the multifunctional polymer additive of the present invention can be adsorbed on the electrode surface through the association of functional monomers with electrode fibers, improving the electrochemical reversibility and kinetics of the redox couple on the electrode, thereby improving the efficiency of the vanadium battery. The voltage and energy efficiency of the battery stack of Comparative Example 1 are higher than those of the blank group Comparative Example 4 but lower than those of Example 1. This is because the free radical polymerization preparation cannot achieve the concentration of functional monomers in the polymer chain segments, which weakens the association and thus limits the modification of the electrode fibers. The battery stack performances of Comparative Example 2, Comparative Example 3 and Comparative Example 4 are similar. This is because Comparative Example 2 and Comparative Example 3 have no functional monomers and cannot be loaded on the surface of the electrode fibers through the association to improve the electrochemical activity of the electrode.

[0039] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a multifunctional polymer additive for vanadium electrolyte, characterized in that: The following steps are involved: Step S1, weighing 3-9 parts by weight of a reversible addition-fragmentation chain transfer reagent, 10-30 parts by weight of a carboxyl or amino monomer, 100-150 parts by weight of deionized water and 0.2-0.6 parts of an initiator, mixing and stirring to dissolve, introducing nitrogen and heating to 70-85° C., reacting for 1.5-3 hours, to obtain a mixed solution 1; Step S2, weigh 5-30 parts by weight of sulfonic acid monomer, 40-80 parts by weight of deionized water and 0.2-0.6 parts by weight of initiator, mix and stir to dissolve, add to the mixed solution 1, heat to 75-90° C., react for 1.5-3 hours, and obtain the mixed solution 2; Step S3, weigh 0.5-1 parts by weight of functional monomer, 10-20 parts by weight of deionized water and 0.05-0.1 parts by weight of initiator, mix and stir to dissolve, then add to the mixed solution, heat to 75-90° C., react for 8-12 hours, and obtain a mixed solution III; Step S4, filtering the mixed solution, vacuum drying at 30-40° C. for 12-18 h and grinding with a mortar to obtain a multifunctional polymer additive.

2. The method for preparing a multifunctional polymer additive for vanadium electrolyte according to claim 1, characterized in that: In step S1, the reversible addition-fragmentation chain transfer reagent is any one of 2-[(dodecylsulfanyl)thioacyl]-sulfanylpropionic acid, dithiophenylacetate pyridinium chloride, S-(2-propionic acid)-S'-(2-methylpropionic acid) trithiocarbonate, and dithiobenzoate pyridinium chloride.

3. The method for preparing a multifunctional polymer additive for vanadium electrolyte according to claim 1, characterized in that: In step S1, the carboxyl or amino monomer is any one of acrylic acid, methacrylic acid, itaconic acid, acrylamide, methacrylamide, and hydroxymethyl acrylamide.

4. The method for preparing a multifunctional polymer additive for vanadium electrolyte according to claim 1, characterized in that: In steps S1, S2 and S3, the initiator is any one of azobiscyanovaleric acid, ammonium persulfate, sodium persulfate and potassium persulfate.

5. The method for preparing a multifunctional polymer additive for vanadium electrolyte according to claim 1, characterized in that: In step S2, the sulfonic acid monomer is any one of sodium methyl methacrylate sulfonate, sodium p-styrene sulfonate, and 2-acrylamide-2-methylpropane sulfonic acid.

6. The method for preparing a multifunctional polymer additive for vanadium electrolyte according to claim 1, characterized in that: The functional monomer in step S3 is any one of tristyrylphenol polyethylene glycol methacrylate BOM25, alkoxy polyethylene glycol methacrylate BOM60, and double-bond-containing urea heterocyclic compound V-70M.

7. The method for preparing a multifunctional polymer additive for vanadium electrolyte according to claim 1, characterized in that: The viscosity average molecular weight of the multifunctional polymer additive in step S4 is 1000-10000.

8. A multifunctional polymer additive for vanadium electrolyte, characterized in that: The multifunctional polymer additive is prepared by the method for preparing a multifunctional polymer additive for vanadium electrolyte as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Preparation method of water-dispersible polyacrylamide polymer

    CN110156925A

  • Binder material for improving low-temperature performance of lithium battery and preparation method of binder material

    CN113644266A

  • Multi-block polycarboxylic acid dispersing agent as well as preparation method and application thereof

    CN118725215A

  • Film for medicine packaging and method of preparing the same

    US20200070485A1