Preparation method of bio-based high-toughness polyurethane elastomer and polyurethane fiber
By using bio-based polylactide diol and high-density hydrogen bonds in polyurethane elastomers, combining non-covalent interactions, the contradiction between strength and toughness of polyurethane elastomers is solved, and the high strength and toughness of the material are achieved , repairable, recyclable and degradable properties, extend service life and reduce resource waste and pollution.
Patent Information
- Application Number
- CN202411136003.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
AI Technical Summary
There is a contradiction between strength and toughness of existing polyurethane elastomers, and it is difficult to repair, recycle, and degrade, resulting in waste of resources and pollution.
Using bio-based high-strength polyurethane elastomers and fibers, the polyol is preferably polylactide diol, and high-density hydrogen bonds are introduced, and non-covalent interactions are used as crosslinking sites to impart repairable and recyclable materials. , degradable properties.
It achieves high strength and toughness of polyurethane elastomers and fibers, and extends the service life of the material. The material can be self-healed at 60-120℃ and completely degraded in the natural environment, solving the problems of resource waste and pollution.
Smart Images

Figure CN118909223A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane elastomers, and in particular relates to a preparation method of a bio-based high-strength polyurethane elastomer and polyurethane fiber. Background Art
[0002] Polyurethane elastomers are generally composed of two phases, soft and hard. The soft segment is usually composed of macromolecular polyols, and the hard segment is often composed of isocyanates and chain extenders. By adjusting the soft and hard segments, the phase separation structure of polyurethane elastomers can be regulated to improve the strength and toughness of the material. Strength and toughness reflect the local performance and failure characteristics of polyurethane elastomers, respectively, but the two are contradictory. With the development of society and the deepening of scientific research, people's demand for synergistically strong polyurethane elastomers has become increasingly strong.
[0003] At the same time, with the development of science and technology, the improvement of human civilization, and the increase in production and living needs, a large amount of materials have been discarded, causing serious waste and pollution. Giving polyurethane elastomers repairable, recyclable, and degradable properties can extend the service life of polyurethane elastomers and reduce resource waste. Summary of the invention
[0004] In order to improve the strength and toughness of polyurethane elastomers and solve the technical problems of difficult repair, difficult recycling and difficult degradation, the present invention provides a bio-based high-strength and tough polyurethane elastomer; the present invention also provides a method for preparing the bio-based high-strength and tough polyurethane elastomer; the present invention also provides a method for preparing the bio-based high-strength and tough polyurethane fiber.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A bio-based high-toughness polyurethane elastomer comprises the following raw materials in percentage by mass: 7.50%-16.50% of polyol, 2.0%-9.50% of isocyanate, 0.20%-6.50% of chain extender, 0.02%-0.04% of catalyst and 78%-89% of solvent.
[0007] Preferably, the polyol is polylactide diol;
[0008] The isocyanate is at least one of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), and dicyclohexylmethane diisocyanate (HMDI);
[0009] The chain extender is at least one of adipic acid dihydrazide (ADH), oxalic acid dihydrazide (ODH), dodecanedicarboxylic acid dihydrazide (DDH), isophthalic acid dihydrazide (IPDH), and 4,4'-diaminobenzanilide (DABA);
[0010] The catalyst is dibutyltin dilaurate;
[0011] The solvent is at least one of N,N-dimethylformamide and N,N-dimethylacetamide.
[0012] A method for preparing the bio-based high-toughness polyurethane elastomer as described in any one of the above comprises the following steps performed in sequence:
[0013] 1) Dehydrate the polyol by vacuum stirring at 100-120°C for 2-4 hours;
[0014] 2) placing polyol, isocyanate and catalyst in a dry solvent and reacting at 60-80°C for 3-6h;
[0015] Then add chain extender and solvent, and react at 40-80°C for 12-15h;
[0016] 3) removing the solvent and molding to obtain a bio-based high-strength and tough polyurethane elastomer.
[0017] Preferably, in step 1), the molecular weight of the polyol is 500-2000.
[0018] Preferably, in step 2), the molar ratio of the polyol to the isocyanate to the chain extender is 1:(1.25-5):(0.25-4).
[0019] A method for preparing bio-based high-toughness polyurethane fiber, comprising spinning any of the above-mentioned bio-based high-toughness polyurethane elastomers or a polyurethane elastomer prepared by any of the above-mentioned methods for preparing a bio-based high-toughness polyurethane elastomer, to obtain bio-based high-toughness polyurethane fiber;
[0020] The spinning is at least one of melt spinning, dry spinning, dry-jet wet spinning and wet spinning.
[0021] Preferably, the melt spinning is specifically: extruding, spinning, cooling, drawing and winding the polyurethane elastomer in sequence to obtain polyurethane fibers;
[0022] The spinning temperature is 160-220° C., and the spinning rate is 400-1000 m / min.
[0023] Preferably, the dry spinning method specifically comprises: subjecting the polyurethane elastomer to rotary evaporation, filtration, degassing, spinning, drawing, and winding in sequence, and obtaining polyurethane fibers after completion;
[0024] The mass percentage concentration of the spinning solution is 25% to 35%, the spinning temperature is 200 to 230° C., and the spinning speed is 200 to 600 m / min.
[0025] Preferably, the dry-jet wet spinning method comprises: sequentially subjecting the polyurethane elastomer solution to rotary evaporation, filtration, degassing, spinning, coagulation in a coagulation bath, drawing, and winding, and after completion, polyurethane fibers are obtained;
[0026] The mass percentage concentration of the spinning solution is 25% to 35%, the spinning temperature is 200 to 230°C, the spinning rate is 200 to 600 m / min, the air layer gap is 3 to 20 mm, and the coagulation bath is an aqueous solution containing 0% to 30% solvent and 0% to 20% metal ions.
[0027] Preferably, the wet spinning method specifically comprises: subjecting the polyurethane elastomer solution to rotary evaporation, filtration, degassing, spinning, coagulation in a coagulation bath, drawing, and winding in sequence, and after completion, polyurethane fibers are obtained;
[0028] The mass percentage concentration of the spinning solution is 15% to 25%, the spinning temperature is 20 to 40° C., the spinning rate is 50 to 150 m / min, and the coagulation bath is an aqueous solution containing 0% to 30% solvent and 0% to 20% metal ions.
[0029] Compared with the prior art, the present invention has the following advantages and technical effects:
[0030] (1) The present invention optimizes the polyol structure from the perspective of TPU structure, uses biodegradable bio-based polylactide diol, and gives the polyurethane elastomer a new degradable function; the high-strength polyurethane elastomer and polyurethane fiber provided by the present invention have a bio-based content of more than 70%.
[0031] (2) The polyurethane elastomer and polyurethane fiber obtained by the preparation method provided by the present invention have high strength and high toughness. The present invention introduces high-density hydrogen bonds in the TPU hard segment structure, thereby achieving the strengthening and toughening effects of the material. The strain of the film material of the polyurethane elastomer of the present invention exceeds 1400%, and the breaking strength is as high as 66MPa; the strain of the polyurethane fiber exceeds 800%, and the breaking strength is as high as 214MPa.
[0032] (3) The bio-based content in the polyurethane elastomer and polyurethane fiber of the present invention can be adjusted according to different requirements and can be higher than 80%.
[0033] (4) The present invention selects non-covalent interactions as cross-linking sites and introduces them into the polyurethane elastomer, thereby giving the polyurethane elastomer self-healing and recycling properties, thereby extending the material's service stability and life; after the bio-based high-strength polyurethane elastomer of the present invention is mechanically damaged, its fracture surfaces can be joined and heated at 60 to 120°C to achieve self-repair; the bio-based high-strength polyurethane elastomer of the present invention can also be recycled by re-dissolving in a solvent.
[0034] (5) The present invention selects bio-based polylactide diol as raw material, and the synthesized polyurethane elastomer is biodegradable. The bio-based polyurethane elastomer of the present invention is buried in the soil of the natural environment (300mm 3 ), and it can be completely degraded after 6 months. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is the stress-strain curve of the bio-based high-toughness polyurethane elastomer film in Example 1;
[0036] Figure 2 is the stress-strain curve of the bio-based high-toughness polyurethane fiber in Example 2;
[0037] Figure 3 is the stress-strain curve of the bio-based high-toughness polyurethane fiber in Example 3;
[0038] Figure 4 is the stress-strain curve of the polyurethane fiber in Comparative Example 1;
[0039] Figure 5 is the stress-strain curve of the polyurethane fiber in Comparative Example 2;
[0040] Figure 6 This is the stress-strain curve of the polyurethane fiber in Comparative Example 3. DETAILED DESCRIPTION
[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of them. Therefore, based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] The present application provides a bio-based high-toughness polyurethane elastomer, comprising the following raw materials in percentage by mass: 7.50%-16.50% of polyol, 2.0%-9.50% of isocyanate, 0.20%-6.50% of chain extender, 0.02%-0.04% of catalyst, and 78%-89% of solvent; preferably, 7.76%-16.25% of polyol, 2.26%-9.12% of isocyanate, 0.26%-6.03% of chain extender, 0.02% of catalyst, and 78%-89% of solvent.
[0043] In one embodiment of the present application, the polyol is polylactide diol;
[0044] The isocyanate is at least one of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), and dicyclohexylmethane diisocyanate (HMDI);
[0045] The chain extender is at least one of adipic acid dihydrazide (ADH), oxalic acid dihydrazide (ODH), dodecanedicarboxylic acid dihydrazide (DDH), isophthalic acid dihydrazide (IPDH), and 4,4'-diaminobenzanilide (DABA);
[0046] The catalyst is dibutyltin dilaurate;
[0047] The solvent is at least one of N,N-dimethylformamide and N,N-dimethylacetamide.
[0048] The present application provides a method for preparing a bio-based high-toughness polyurethane elastomer, comprising the following steps performed in sequence:
[0049] 1) Dehydrate the polyol by vacuum stirring at 100-120°C for 2-4 hours;
[0050] 2) placing polyol, isocyanate and catalyst in a dry solvent and reacting at 60-80°C for 3-6h;
[0051] Then add chain extender and solvent, and react at 40-80°C for 12-15h;
[0052] 3) removing the solvent and molding to obtain a bio-based high-strength and tough polyurethane elastomer.
[0053] In one embodiment of the present application, in step 1), the molecular weight of the polyol is 500-2000, preferably 1000.
[0054] In one embodiment of the present application, in step 2), the molar ratio of the polyol to the isocyanate to the chain extender is 1:(1.25-5):(0.25-4), preferably 1:1.5:0.5.
[0055] In the present application, in step 3), the solvent is removed in an oven, and the polymer from which the solvent has been removed is subjected to extrusion, hot pressing or other processes to shape the material, thereby obtaining the bio-based high-strength and tough polyurethane elastomer.
[0056] The present application provides a method for preparing a bio-based high-toughness polyurethane fiber, wherein the bio-based high-toughness polyurethane elastomer described in any one of the above or the polyurethane elastomer prepared by the method for preparing a bio-based high-toughness polyurethane elastomer described in any one of the above is spun to obtain a bio-based high-toughness polyurethane fiber;
[0057] The spinning is at least one of melt spinning, dry spinning, dry-jet wet spinning and wet spinning.
[0058] In one embodiment of the present application, the melt spinning is specifically: extruding, spinning, cooling, drawing, and winding the polyurethane elastomer in sequence to obtain polyurethane fibers;
[0059] The spinning temperature is 160-220° C., and the spinning rate is 400-1000 m / min.
[0060] In one embodiment of the present application, the dry spinning method specifically comprises: sequentially performing rotary evaporation, filtering, degassing, spinning, drawing, and winding on the polyurethane elastomer to obtain polyurethane fibers;
[0061] The mass percentage concentration of the spinning solution is 25% to 35%, the spinning temperature is 200 to 230° C., and the spinning speed is 200 to 600 m / min.
[0062] In one embodiment of the present application, the dry-jet wet spinning method is specifically as follows: the polyurethane elastomer solution is subjected to rotary evaporation, filtration, degassing, spinning, coagulation in a coagulation bath, drawing, and winding in sequence, and polyurethane fibers are obtained after completion;
[0063] The mass percentage concentration of the spinning solution is 25% to 35%, the spinning temperature is 200 to 230°C, the spinning rate is 200 to 600 m / min, the air layer gap is 3 to 20 mm, and the coagulation bath is an aqueous solution containing 0% to 30% solvent and 0% to 20% metal ions.
[0064] In one embodiment of the present application, the wet spinning method specifically comprises: sequentially performing rotary evaporation, filtration, degassing, spinning, coagulation in a coagulation bath, drawing, and winding on the polyurethane elastomer solution, and obtaining the polyurethane fiber after completion;
[0065] The mass percentage concentration of the spinning solution is 15% to 25%, the spinning temperature is 20 to 40° C., the spinning rate is 50 to 150 m / min, and the coagulation bath is an aqueous solution containing 0% to 30% solvent and 0% to 20% metal ions.
[0066] In the present application, the metal ions in the aqueous solution containing metal ions include but are not limited to Zn 2+ , Cu 2+ , Ca 2 + ,Mg 2+ , Fe 2+ , Fe 3+ , Ag + ,Co 2+ , Ni 2+ At least one of .
[0067] The present invention introduces hydrazide raw materials into the hard segment of the polyurethane elastomer, which reacts with isocyanate groups to generate acyl semicarbazide groups, forming a high-density hydrogen bond network, thereby improving the strength and toughness of the material; at the same time, the hydrogen bond cross-linked network of the elastomer can be dynamically dissociated and reorganized, so that the elastomer has repairable and recyclable properties; and the bio-based raw material-polylactide diol is used as the polymer matrix to give the polyurethane elastomer biodegradability.
[0068] The polyurethane elastomer synthesized with polylactide diol as raw material proposed by the present invention is not only biodegradable, but also easy to recycle and reprocess, which can solve the white pollution and resource waste caused by non-degradable materials. With bio-based polylactide diol as the soft segment and non-covalent interaction as the cross-linking site, a polyurethane elastomer material with high strength, high toughness, repairability, recyclability and degradability is prepared. The strain of the polyurethane elastomer of the present invention exceeds 1400%, the breaking strength is as high as 66MPa, the product performance is excellent, and the bio-based component is greater than 70%. The strain of the polyurethane fiber of the present invention exceeds 800%, and the breaking strength is as high as 214MPa.
[0069] The methods and devices not described in detail in the present invention are all prior art and will not be described in detail.
[0070] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0071] Example 1
[0072] A bio-based high-strength polyurethane elastomer is made from the following raw materials in percentage by weight:
[0073] 8.77% polyol, 2.93% isocyanate, 0.52% chain extender, 0.02% catalyst, 87.76% solvent;
[0074] The polyol is polylactide diol with a molecular weight of 1000;
[0075] The chain extender is oxalic acid dihydrazide;
[0076] The isocyanate is isophorone diisocyanate;
[0077] The total biobased content of the system is 71.8%.
[0078] A method for preparing a bio-based high-toughness polyurethane elastomer according to Example 1 comprises the following steps performed in sequence:
[0079] 1) Dehydrate the polyol by stirring under vacuum at 110°C for 2 h;
[0080] 2) placing polyol, isocyanate and catalyst in a dry solvent and reacting at 80°C for 3h;
[0081] Then, a chain extender and a solvent were added and reacted at 60°C for 12 h;
[0082] 3) removing the solvent and molding to obtain a bio-based high-strength and tough polyurethane elastomer.
[0083] Example 2
[0084] A bio-based high-strength polyurethane elastomer is made from the following raw materials in percentage by weight:
[0085] 8.77% polyol, 2.93% isocyanate, 0.52% chain extender, 0.02% catalyst, 87.76% solvent;
[0086] The polyol is polylactide diol with a molecular weight of 1000;
[0087] The chain extender is oxalic acid dihydrazide;
[0088] The isocyanate is isophorone diisocyanate;
[0089] The total biobased content of the system is 71.8%.
[0090] A method for preparing a bio-based high-toughness polyurethane elastomer according to Example 2 comprises the following steps performed in sequence:
[0091] 1) Dehydrate the polyol by stirring under vacuum at 110°C for 2 h;
[0092] 2) placing polyol, isocyanate and catalyst in a dry solvent and reacting at 80°C for 3h;
[0093] Then, a chain extender and a solvent were added and the reaction was carried out at 60° C. for 12 h.
[0094] A method for preparing a bio-based high-strength polyurethane fiber in Example 2, wherein the bio-based high-strength polyurethane elastomer solution is subjected to wet spinning, and the specific steps are: rotary evaporation, filtration, degassing, spinning, coagulation in a coagulation bath, drawing, and winding, and after completion, the bio-based high-strength polyurethane fiber is obtained;
[0095] The mass percentage concentration of the spinning solution is 20%, the spinning temperature is 25° C., the spinning speed is 50 m / min, and the coagulation bath is an aqueous solution containing 30% of the solvent.
[0096] Example 3
[0097] A bio-based high-strength polyurethane elastomer is made from the following raw materials in percentage by weight:
[0098] 8.77% polyol, 2.93% isocyanate, 0.52% chain extender, 0.02% catalyst, 87.76% solvent;
[0099] The polyol is polylactide diol with a molecular weight of 1000;
[0100] The chain extender is oxalic acid dihydrazide;
[0101] The isocyanate is isophorone diisocyanate;
[0102] The total biobased content of the system is 71.8%.
[0103] The method for preparing the bio-based high-toughness polyurethane elastomer of Example 3 comprises the following steps performed in sequence:
[0104] 1) Dehydrate the polyol by stirring under vacuum at 110°C for 2 h;
[0105] 2) placing polyol, isocyanate and catalyst in a dry solvent and reacting at 80°C for 3h;
[0106] Then, a chain extender and a solvent were added and the reaction was carried out at 60° C. for 12 h.
[0107] A method for preparing a bio-based high-toughness polyurethane fiber in Example 3, wherein the bio-based high-toughness polyurethane elastomer solution is subjected to wet spinning, and the specific steps are: rotary evaporation, filtration, degassing, spinning, coagulation in a coagulation bath, drawing, and winding, and the bio-based high-toughness polyurethane fiber is obtained after completion;
[0108] The mass percentage concentration of the spinning solution is 20%, the spinning temperature is 25° C., the spinning rate is 50 m / min, and the coagulation bath is an aqueous solution containing 30% solvent and 0.5% ZnCl2.
[0109] Comparative Example 1
[0110] Polyurethane elastomer, made from the following raw materials in percentage by mass:
[0111] 8.84% polyol, 2.46% isocyanate, 0.26% chain extender, 0.02% catalyst, 88.42% solvent;
[0112] The polyol is polylactide diol with a molecular weight of 1000;
[0113] The chain extender is oxalic acid dihydrazide;
[0114] The isocyanate is isophorone diisocyanate;
[0115] The total biobased content of the system is 76.49%.
[0116] The preparation method of the polyurethane elastomer of Comparative Example 1 comprises the following steps performed in sequence:
[0117] 1) Dehydrate the polyol by stirring under vacuum at 110°C for 2 h;
[0118] 2) placing polyol, isocyanate and catalyst in a dry solvent and reacting at 80°C for 3h;
[0119] Then, a chain extender and a solvent were added and the reaction was carried out at 60° C. for 12 h.
[0120] The preparation method of the polyurethane fiber of Comparative Example 1 is to wet-spin the polyurethane elastomer solution, and the specific steps are: rotary evaporation, filtration, degassing, spinning, coagulation in a coagulation bath, drawing, and winding, and then obtain the polyurethane fiber;
[0121] The mass percentage concentration of the spinning solution is 20%, the spinning temperature is 25° C., the spinning rate is 50 m / min, and the coagulation bath is an aqueous solution containing 30% solvent and 0.5% ZnCl2.
[0122] Comparative Example 2
[0123] Polyurethane elastomer, made from the following raw materials in percentage by mass:
[0124] 7.95% polyol, 8.83% isocyanate, 3.75% chain extender, 0.02% catalyst, 79.45% solvent;
[0125] The polyol is polylactide diol with a molecular weight of 1000;
[0126] The chain extender is oxalic acid dihydrazide;
[0127] The isocyanate is isophorone diisocyanate;
[0128] The total biobased content of the system is 38.7%.
[0129] The preparation method of the polyurethane elastomer of Comparative Example 2 comprises the following steps performed in sequence:
[0130] 1) Dehydrate the polyol by stirring under vacuum at 110°C for 2 h;
[0131] 2) placing polyol, isocyanate and catalyst in a dry solvent and reacting at 80°C for 3h;
[0132] Then, a chain extender and a solvent were added and the reaction was carried out at 60° C. for 12 h.
[0133] The preparation method of the polyurethane fiber of Comparative Example 2 is to wet-spin the polyurethane elastomer solution, and the specific steps are: rotary evaporation, filtration, degassing, spinning, coagulation in a coagulation bath, drawing, and winding, and then obtain the polyurethane fiber;
[0134] The mass percentage concentration of the spinning solution is 20%, the spinning temperature is 25° C., the spinning rate is 50 m / min, and the coagulation bath is an aqueous solution containing 30% solvent and 0.5% ZnCl2.
[0135] Comparative Example 3
[0136] The comparative example 3 is a commercially available polyurethane fiber.
[0137] Performance Testing
[0138] The polyurethane elastomer films and polyurethane fiber products obtained in Examples 1-3 and Comparative Examples 1-3 were subjected to mechanical property tests according to the following standards. The results are shown in Table 1.
[0139] Mechanical properties: Data provided by universal material testing machine (Instron5965), test conditions are room temperature, -20% relative humidity, tensile speed is 50mmmin -1 The film tensile specimens were dumbbell-shaped (width: 2 mm; length: 12 mm), and the fiber tensile specimens were 5 cm long.
[0140] Table 1 Performance test data of polyurethane materials prepared in Examples and Comparative Examples
[0141]
[0142]
[0143] It can be seen from the test data in Table 1 that the bio-based high-toughness polyurethane elastomer and polyurethane fiber of the present invention can achieve a bio-based content of more than 70%;
[0144] By comparing Example 3 with Comparative Example 1, the introduction of high-density hydrogen bonds can improve the strength and toughness of the polyurethane elastomer;
[0145] By comparing Example 3 with Comparative Example 2, excessive hydrogen bonding will lead to excessive crosslinking density, which will reduce the mechanical properties.
[0146] By comparing Example 3 with Comparative Example 3, the bio-based polyurethane fiber proposed by the present invention has a strength of 3.5 times and a toughness of 7 times that of commercially available polyurethane fibers.
[0147] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A bio-based high-toughness polyurethane elastomer, characterized in that: The invention comprises the following raw materials in percentage by mass: 7.50%-16.50% of polyol, 2.0%-9.50% of isocyanate, 0.20%-6.50% of chain extender, 0.02%-0.04% of catalyst and 78%-89% of solvent.
2. A bio-based high-toughness polyurethane elastomer according to claim 1, characterized in that: The polyol is polylactide diol; The isocyanate is at least one of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), and dicyclohexylmethane diisocyanate (HMDI); The chain extender is at least one of adipic acid dihydrazide (ADH), oxalic acid dihydrazide (ODH), dodecanedicarboxylic acid dihydrazide (DDH), isophthalic acid dihydrazide (IPDH), and 4,4'-diaminobenzanilide (DABA); The catalyst is dibutyltin dilaurate; The solvent is at least one of N,N-dimethylformamide and N,N-dimethylacetamide.
3. A method for preparing a bio-based high-toughness polyurethane elastomer according to any one of claims 1 to 2, characterized in that: The method includes the following steps: 1) Dehydrate the polyol by vacuum stirring at 100-120°C for 2-4 hours; 2) placing polyol, isocyanate and catalyst in a dry solvent and reacting at 60-80°C for 3-6h; Then add chain extender and solvent, and react at 40-80°C for 12-15h; 3) removing the solvent and molding to obtain a bio-based high-strength and tough polyurethane elastomer.
4. The method for preparing a bio-based high-toughness polyurethane elastomer according to claim 3, characterized in that: In step 1), the molecular weight of the polyol is 500-2000.
5. The method for preparing a bio-based high-toughness polyurethane elastomer according to claim 3, characterized in that: In step 2), the molar ratio of the polyol to the isocyanate to the chain extender is 1:(1.25-5):(0.25-4).
6. A method for preparing bio-based high-strength polyurethane fiber, characterized in that: Spinning the bio-based high-toughness polyurethane elastomer according to any one of claims 1 to 2 or the polyurethane elastomer prepared by the method for preparing the bio-based high-toughness polyurethane elastomer according to any one of claims 3 to 5 to obtain bio-based high-toughness polyurethane fibers; The spinning is at least one of melt spinning, dry spinning, dry-jet wet spinning and wet spinning.
7. The method for preparing bio-based high-toughness polyurethane fiber according to claim 6, characterized in that: The melt spinning specifically comprises: extruding, spinning, cooling, drawing and winding the polyurethane elastomer in sequence, and obtaining polyurethane fibers after completion; The spinning temperature is 160-220° C., and the spinning rate is 400-1000 m / min.
8. The method for preparing bio-based high-toughness polyurethane fiber according to claim 6, characterized in that: The dry spinning method specifically comprises: sequentially performing rotary evaporation, filtering, degassing, spinning, drawing and winding on the polyurethane elastomer to obtain polyurethane fibers; The mass percentage concentration of the spinning solution is 25% to 35%, the spinning temperature is 200 to 230° C., and the spinning speed is 200 to 600 m / min.
9. The method for preparing bio-based high-toughness polyurethane fiber according to claim 6, characterized in that: The dry-jet wet spinning method specifically comprises: sequentially performing rotary evaporation, filtering, degassing, spinning, coagulation in a coagulation bath, drawing, and winding on the polyurethane elastomer solution, and obtaining polyurethane fibers after completion; The mass percentage concentration of the spinning solution is 25% to 35%, the spinning temperature is 200 to 230°C, the spinning rate is 200 to 600 m / min, the air layer gap is 3 to 20 mm, and the coagulation bath is an aqueous solution containing 0% to 30% solvent and 0% to 20% metal ions.
10. The method for preparing bio-based high-toughness polyurethane fiber according to claim 6, characterized in that: The wet spinning method specifically comprises: sequentially subjecting the polyurethane elastomer solution to rotary evaporation, filtration, degassing, spinning, coagulation in a coagulation bath, drawing, and winding, and finally obtaining polyurethane fibers; The mass percentage concentration of the spinning solution is 15% to 25%, the spinning temperature is 20 to 40° C., the spinning rate is 50 to 150 m / min, and the coagulation bath is an aqueous solution containing 0% to 30% solvent and 0% to 20% metal ions.
Citation Information
Patent Citations
A method for preparing a super-tough polyurethane crosslinked network
CN114933723A
Preparation method of polylactic acid-based polyurethane elastic fiber
CN117568951A
Ultra-high-performance transparent self-repairing polyurethane-urea film capable of being recycled repeatedly and preparation method of ultra-high-performance transparent self-repairing polyurethane-urea film
CN117624538A
Cited By
Method for continuously manufacturing high-strength and high-toughness protein-like fibers
CN119640417A
Preparation method and application of bio-based high-strength and high-toughness polyurethane
CN119955061A