High-strength spandex fiber and preparation method thereof
By introducing regenerated cellulose into spandex fibers and regulating the reaction of prepolymers, high-strength and high heat-resistant spandex fibers are prepared, which solves the problem of insufficient strength and heat resistance of spandex fibers, and reduces carbon emissions and achieves high Value-added textile performance.
Patent Information
- Application Number
- CN202411200453.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The insufficient strength and heat resistance of existing spandex fibers limit their use in high-demand applications. At the same time, their production process relies on petrochemical resources, resulting in carbon emission problems and is difficult to meet the requirements of green development.
By introducing regenerated cellulose into the spandex macromolecular chain, the molar ratio of polydiol and diisocyanate is regulated, the chain extender and regenerated cellulose/LiCl solution are added for mixing reaction, forming a high molecular weight prepolymer. Dry spinning to prepare high-strength spandex fibers to increase their mechanical properties and natural cellulose components.
It significantly improves the mechanical properties and thermal stability of spandex fibers, meets the application needs of industrial textiles and aerospace and military industries, and at the same time reduces carbon emissions and gives textiles excellent comfort and model-resistance performance.
Smart Images

Figure CN118909224A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer fiber material preparation, and in particular to a high-strength spandex fiber and a preparation method thereof. Background Art
[0002] Spandex has an incomparable elasticity compared to other synthetic fibers. Its elongation at break is as high as 800%, and its elastic recovery rate is over 95%. It is widely used in textiles and clothing, medical and health care, sports, national defense and military industries, etc. A small amount of addition can give textiles excellent elasticity, comfort and shape retention. It is an indispensable fiber material for high-end textiles. At the same time, it is also widely used in the field of disposable sanitary products such as diapers, protective clothing, and nursing products, as well as in the field of sports and leisure.
[0003] Conventional spandex is prepared by polymerization and spinning of polyether polyols and diisocyanates. Due to the presence of a large number of aliphatic polyols in the spandex molecular chain, the molecular chain is relatively flexible. Although it has excellent elasticity, its strength and modulus are low. It is mainly used in the form of core-spun yarn, covered yarn or twisted yarn, which limits the further application of spandex. In addition, the polymer raw materials of spandex are all derived from petrochemical resources, which is not conducive to low carbon emissions and does not meet the requirements of green development of the spandex industry.
[0004] Patent CN 115961397 A discloses a regenerated cellulose fiber spandex core-spun yarn and a processing method thereof; the invention is used to meet the requirements of sportswear for fabric comfort, by selecting soybean fiber and polyurethane fiber in a ratio of 1:1, stirring and mixing at 180-220°C, stirring for 1h, drying and heating at a speed of 10-15°C / min, controlling the heating temperature at 300-320°C, and maintaining for 30min to make a core yarn spandex, selecting raw cotton for opening, carding, drawing and coarse sanding to obtain an outer yarn regenerated cellulose fiber, and then the prepared core yarn and outer yarn are subjected to a fine sanding process to obtain a regenerated cellulose fiber spandex core-spun yarn, by adding regenerated cellulose fiber, the comfort of the spandex core-spun yarn is improved, the water absorption of the spandex core-spun yarn is increased, and the elasticity and toughness of the spandex core-spun yarn are increased, so that the fitness wear is more comfortable, and the advantage of good water absorption of the regenerated cellulose fiber spandex core-spun yarn is achieved. The spandex fibers and plant fibers in the fabric are combined together by weaving, which does not improve the heat resistance of the spandex fibers themselves, and is not suitable for occasions where high spandex strength and heat resistance are required. Summary of the invention
[0005] In view of the structural and performance defects of existing spandex fibers, the present invention provides a high-strength spandex fiber and a preparation method thereof. Regenerated cellulose is introduced into the spandex macromolecular chain through molecular structure design, and a new type of spandex fiber with high strength and heat resistance is developed, which expands the application field of spandex and greatly improves the added value of the product.
[0006] In order to achieve the above object, the technical solution of the present invention is achieved as follows: A high-strength spandex fiber and a preparation method thereof, the steps are as follows: (1) First, a polyol and a diisocyanate are dissolved in an N,N-dimethylacetamide (DMAc) solution at a molar ratio of 1:(1.5-2.5) and reacted at 40-80°C for 60-180 min to prepare an isocyanate-terminated prepolymer solution; then a chain extender is added to obtain a mixed solution A in which the isocyanate group accounts for more than 10 mol% of the terminal group, and the prepolymer accounts for 20-40 wt% of the mixed solution A.
[0007] The high-strength spandex fiber and its preparation method, the polyglycol is a polyether polyol or polyester polyol with a molecular weight of 1000-3000. The polyether glycol is one of polytetrahydrofuran ether glycol, polyethylene glycol, and polypropylene glycol; the polyester glycol is one of polybutylene succinate glycol, polybutylene adipate glycol, and polybutylene sebacate glycol.
[0008] The diisocyanate includes one of the following structures, which is any one of 4,4'-methylenebis(phenyl isocyanate), 1,5-naphthalene diisocyanate, dicyclohexylmethane 4,4'-diisocyanate, toluene diisocyanate and 4,4'-diisocyanato-3,3'-dimethylbiphenyl; the structures are as follows: .
[0009] The chain extender is any one of ethylenediamine, propylenediamine, methylcyclohexanediamine, pentamethylenediamine and p-phenylenediamine, and the amount used is 5-25 mol% of the diisocyanate; the specific structures of the chain extenders are as follows: .
[0010] (2) dissolving regenerated cellulose in a mixed solution of LiCl and DMAc to prepare a mixed solution B; The high-strength spandex fiber and its preparation method, the regenerated cellulose has a polymerization degree of 200-600 and is derived from wood pulp, bamboo pulp, fungus grass, rice straw, wheat straw, and its mass fraction is 1-20%.
[0011] The high-strength spandex fiber and preparation method thereof, wherein the mass fraction of LiCl is 5-12%.
[0012] (3) Finally, the mixed solution A and B are mixed and reacted at a mass ratio of 1-20:1 for 30-90 minutes, and the auxiliary agent is added and then aged; and high-strength spandex is prepared by dry spinning.
[0013] The high-strength spandex fiber and its preparation method, the auxiliary agent is an antioxidant, nanoparticles, stabilizer or flame retardant, and the amount used is 0.1-5wt% of the total mass of the spinning solution.
[0014] The method for preparing bio-based spandex fiber comprises the following steps: the dry spinning is an integral spinning assembly, the number of spinning holes is ≥60, the number of spinning winding heads is ≥2, and the winding speed is 600-1200 m / min.
[0015] The high-strength spandex fiber and its preparation method, the spandex fiber has a fineness of ≥7D, a breaking strength of ≥1.5cN / detx, a breaking elongation of 100-600%, and a thermal decomposition temperature of ≥300°C.
[0016] The present invention has the following beneficial effects: (1) The present invention first prepares an isocyanate-terminated prepolymer solution by conventional polydiol and diisocyanate, and obtains a polyurethane urea solution in which the terminal group CNO accounts for more than 10 mol% after chain extension. The solution is then mixed with a regenerated cellulose / LiCl solution for reaction, and the ratio of the two is adjusted to introduce high molecular weight regenerated cellulose into the spandex molecular chain, thereby further increasing the molecular weight of the spandex and giving the spandex fiber a two-block structure, thereby giving the spandex fiber excellent mechanical properties that are adjustable and controllable within a certain range.
[0017] (2) The spandex fiber involved in the present invention not only has excellent mechanical properties and can meet the application in the fields of industrial textiles, aerospace and military industry, but also contains natural cellulose components, which can significantly reduce carbon emissions and give textiles excellent comfort and shape retention properties, thereby increasing the added value of spandex products. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 This is the stress-strain curve of the high-strength spandex fiber in Example 1.
[0020] Figure 2 This is the surface morphology of the high-strength spandex fiber in Example 1 (magnification 500x).
[0021] Figure 3 This is the thermal weight loss curve of the high-strength spandex fiber in Example 1. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: Polytetramethylene glycol with a molecular weight of 1000 and 1,5-naphthalene diisocyanate were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:1.6 and reacted at 75°C for 70 minutes to prepare an isocyanate-terminated prepolymer solution. Diamine, the amount is 8 mol% of 1,5-naphthalene diisocyanate, to obtain a mixed solution A with an isocyanate ratio of >10 mol%, and a prepolymer ratio of 26 wt%; Then, wood pulp regenerated cellulose with a degree of polymerization of 550 was dissolved in a DMAc solution of LiCl to form a mixed solution B, in which the mass fractions of wood pulp cellulose and LiCl were 1wt% and 6wt%, respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 10:1 for 35 minutes, and 0.1wt% of the total mass of the mixed antioxidant 1076, nano-particle titanium dioxide, light stabilizer 738, and flame retardant melamine cyanurate were added and aged; an integral spinning assembly was used, with 120 spinnerets, 3 spinning winders, and a winding speed of 1100m / min. High-strength spandex with a fineness of 10D was prepared by dry spinning. The stress-strain curve of the obtained high-strength spandex fiber is shown in Figure 1 As shown in Figure 1, its breaking strength is 1.82 cN / detx and its breaking elongation is 228%; the morphology of high-strength spandex fiber is shown in Figure 1. Figure 2 As shown in the figure, the fiber surface is smooth and uniform, and the quality stability is good; the thermal weight loss curve of high-strength spandex fiber is as follows Figure 3 As shown, its initial thermal decomposition temperature is 327°C, which shows excellent thermal stability.
[0024] Example 2 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: Polyethylene glycol with a molecular weight of 2000 and dicyclohexylmethane 4,4'-diisocyanate were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:1.7 and reacted at 60°C for 80 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender methylcyclohexanediamine was added in an amount of 10 mol% of dicyclohexylmethane 4,4'-diisocyanate to obtain a mixed solution A with an isocyanate content of >10 mol% and a prepolymer content of 28 wt%; Then, wood pulp regenerated cellulose with a degree of polymerization of 550 was dissolved in a DMAc solution of LiCl to form a mixed solution B, in which the mass fractions of wood pulp cellulose and LiCl were 5wt% and 7wt%, respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 1:1 for 40 minutes, and 0.5wt% of antioxidant 168, nanoparticle silica, stabilizer 144, and flame retardant dimethyl methylphosphonate were added and then aged; an integral spinning assembly was used, with 80 spinnerets, 4 spinning winders, and a winding speed of 1100m / min. 8D high-strength spandex was prepared by dry spinning.
[0025] Example 3 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: Polypropylene glycol with a molecular weight of 3000 and 4,4'-methylenebis(phenyl isocyanate) were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:1.5 and reacted at 80°C for 60 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender, ethylenediamine, was added in an amount of 5 mol% of 4,4'-methylenebis(phenyl isocyanate) to obtain a mixed solution A with an isocyanate content of >10 mol% and a prepolymer content of 30 wt%; Then, wood pulp regenerated cellulose with a degree of polymerization of 600 was dissolved in a DMAc solution of LiCl to form a mixed solution B, in which the mass fractions of wood pulp cellulose and LiCl were 2wt% and 5wt%, respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 20:1 for 30 minutes, and then 1wt% of antioxidant 3010, nano-particle ferroferric oxide, stabilizer zinc oxide, and flame retardant tritolyl phosphate were added and aged; an integral spinning assembly was used, with 60 spinnerets, 3 spinning winders, and a winding speed of 1000m / min. High-strength spandex with a fineness of 8D was prepared by dry spinning.
[0026] Example 4 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: The polybutylene succinate diol with a molecular weight of 2000 and toluene diisocyanate were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:1.8 and reacted at 65°C for 90 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender pentamethylenediamine was added in an amount of 12 mol% of toluene diisocyanate to obtain a mixed solution A with an isocyanate ratio of >10 mol% and a prepolymer ratio of 22wt%; Then, wood pulp regenerated cellulose with a degree of polymerization of 400 was dissolved in a DMAc solution of LiCl to form a mixed solution B, in which the mass fractions of wood pulp cellulose and LiCl were 8wt% and 8wt%, respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 15:1 for 45 minutes, and then 2.5wt% of antioxidant 1076, nano-particle silica, stabilizer zinc oxide, and flame retardant melamine cyanurate were added and aged; an integral spinning assembly was used, with 60 spinnerets, 3 spinning winders, and a winding speed of 600m / min. High-strength spandex with a fineness of 30D was prepared by dry spinning.
[0027] Example 5 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: Polybutylene adipate diol with a molecular weight of 3000 and 4,4'-diisocyanato-3,3'-dimethylbiphenyl were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:1.9 and reacted at 45°C for 100 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender p-phenylenediamine was added in an amount of 15 mol% of 4,4'-diisocyanato-3,3'-dimethylbiphenyl to obtain a mixed solution A with an isocyanate ratio of >10 mol% and a prepolymer ratio of 20wt%; Then, wood pulp regenerated cellulose with a degree of polymerization of 450 is dissolved in a DMAc solution of LiCl to form a mixed solution B; the mass fractions of wood pulp cellulose and LiCl are 10wt% and 9wt% respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 8:1 for 50 minutes, and 1.5wt% of antioxidant 168, nano-particle ferroferric oxide, light stabilizer 783, and flame retardant dimethyl methylphosphonate were added and then aged; an integral spinning assembly was used, with 80 spinnerets, 5 spinning winders, and a winding speed of 800m / min. High-strength spandex with a fineness of 20D was prepared by dry spinning.
[0028] Example 6 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: The polybutylene sebacate diol with a molecular weight of 2000 and 4,4'-methylenebis(phenyl isocyanate) were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:2 and reacted at 50°C for 110 minutes to prepare an isocyanate-terminated prepolymer solution, and p-phenylenediamine, a chain extender, was added in an amount of 18 mol% of 4,4'-methylenebis(phenyl isocyanate) to obtain a mixed solution A with an isocyanate content of >10 mol% and a prepolymer content of 34 wt%; Then, wood pulp regenerated cellulose with a polymerization degree of 300 is dissolved in a DMAc solution of LiCl to form a mixed solution B; the mass fractions of wood pulp cellulose and LiCl are 12wt% and 10wt% respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 4:1 for 55 minutes, and 2wt% of antioxidant 3010, nano-particle titanium dioxide, light stabilizer 144, and flame retardant tricresyl phosphate were added and then aged; an integral spinning assembly was used, with 100 spinnerets, 2 spinning winders, and a winding speed of 600m / min. High-strength spandex with a fineness of 40D was prepared by dry spinning.
[0029] Example 7 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: The polybutylene succinate diol with a molecular weight of 1000 and 1,5-naphthalene diisocyanate were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:2.1 and reacted at 55°C for 120 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender pentamethylenediamine was added in an amount of 20 mol% of 1,5-naphthalene diisocyanate to obtain a mixed solution A with an isocyanate ratio of >10 mol% and a prepolymer ratio of 40wt%; Then, wood pulp regenerated cellulose with a degree of polymerization of 350 was dissolved in a DMAc solution of LiCl to form a mixed solution B; the mass fractions of wood pulp cellulose and LiCl were 16wt% and 12wt%, respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 3:1 for 65 minutes, and 2.8wt% of antioxidant 1076, nano-particle ferric oxide, light stabilizer 144, and flame retardant tricresyl phosphate were added and then aged; an integral spinning assembly was used, with 70 spinnerets, 4 spinning winders, and a winding speed of 1100m / min. High-strength spandex with a fineness of 15D was prepared by dry spinning.
[0030] Example 8 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: The polybutylene succinate diol with a molecular weight of 2000 and dicyclohexylmethane 4,4'-diisocyanate were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:2.2 and reacted at 40°C for 130 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender methylcyclohexanediamine was added in an amount of 22 mol% of dicyclohexylmethane 4,4'-diisocyanate to obtain a mixed solution A with an isocyanate content of >10 mol% and a prepolymer content of 38 wt%; Then, wood pulp regenerated cellulose with a polymerization degree of 250 is dissolved in a DMAc solution of LiCl to form a mixed solution B; the mass fractions of wood pulp cellulose and LiCl are 16wt% and 12wt%, respectively; The mixed solution A and B were mixed and reacted in a mass ratio of 3:1 for 65 minutes, and then 2.8wt% of antioxidant 168, nanoparticle titanium dioxide, light stabilizer 144, and flame retardant melamine cyanurate were added and matured. An integral spinning assembly was used with 70 spinnerets, 4 spinning winding heads, and a winding speed of 600m / min, and high-strength spandex with a fineness of 30D was prepared by dry spinning.
[0031] Example 9 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: The polybutylene sebacate diol with a molecular weight of 2000 and toluene diisocyanate were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:2.3 and reacted at 57°C for 140 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender propylene diamine was added in an amount of 25 mol% of toluene diisocyanate to obtain a mixed solution A with an isocyanate ratio of >10 mol% and a prepolymer ratio of 36 wt%; Then, wood pulp regenerated cellulose with a polymerization degree of 200 is dissolved in a LiCl DMAc solution to form a mixed solution B; the mass fractions of wood pulp cellulose and LiCl are 18wt% and 10wt% respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 15:1 for 70 minutes, and then 3wt% of antioxidant 3010, nanoparticle silica, light stabilizer 783, and flame retardant tricresyl phosphate were added and aged. An integral spinning assembly was used with 80 spinnerets, 4 spinning winders, and a winding speed of 1100m / min, and high-strength spandex with a fineness of 10D was prepared by dry spinning.
[0032] Example 10 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: Polypropylene glycol with a molecular weight of 1500 and 4,4'-diisocyanato-3,3'-dimethylbiphenyl were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:2.5 and reacted at 63°C for 150 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender ethylenediamine was added in an amount of 21 mol% of 4,4'-diisocyanato-3,3'-dimethylbiphenyl to obtain a mixed solution A with an isocyanate ratio of >10 mol%; Then, wood pulp regenerated cellulose with a polymerization degree of 300 is dissolved in a DMAc solution of LiCl to form a mixed solution B; the mass fractions of wood pulp cellulose and LiCl are 20wt% and 8wt% respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 18:1 for 75 minutes, and 3.5wt% of antioxidant, nanoparticles, stabilizer and flame retardant were added and then aged; an integral spinning assembly was used with 90 spinnerets, 3 spinning winding heads and a winding speed of 1000m / min, and high-strength spandex was prepared by dry spinning.
[0033] Embodiment 11 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: Polyethylene glycol with a molecular weight of 2500 and 4,4'-methylenebis(phenyl isocyanate) were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:1.5 and reacted at 80°C for 60 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender, ethylenediamine, was added in an amount of 5 mol% of 4,4'-methylenebis(phenyl isocyanate) to obtain a mixed solution A with an isocyanate content of >10 mol% and a prepolymer content of 26 wt%; Then, wood pulp regenerated cellulose with a polymerization degree of 600 is dissolved in a LiCl DMAc solution to form a mixed solution B; the mass fractions of wood pulp cellulose and LiCl are 2wt% and 5wt% respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 20:1 for 30 minutes, and then 1wt% of antioxidant 168, nano-particle titanium dioxide, stabilizer zinc oxide, and flame retardant tricresyl phosphate were added and aged. An integral spinning assembly was used with 60 spinnerets, 3 spinning winding heads, and a winding speed of 1200m / min, and high-strength spandex with a fineness of 7D was prepared by dry spinning.
[0034] Example 12 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: The polybutylene sebacate diol with a molecular weight of 3000 and 4,4'-methylenebis(phenyl isocyanate) were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:2 and reacted at 60°C for 180 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender methylcyclohexanediamine was added in an amount of 23 mol% of 4,4'-methylenebis(phenyl isocyanate) to obtain a mixed solution A with an isocyanate content of >10 mol% and a prepolymer content of 24 wt%; Then, wood pulp regenerated cellulose with a degree of polymerization of 450 is dissolved in LiCl and DMAc solution to form a mixed solution B; the mass fractions of wood pulp cellulose and LiCl are 4wt% and 7wt%, respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 16:1 for 80 minutes, and then 3wt% of antioxidant 3010, nanoparticle titanium dioxide, light stabilizer 783, and flame retardant melamine cyanurate were added and aged. An integral spinning assembly was used with 60 spinnerets, 2 spinning winders, and a winding speed of 1200m / min, and high-strength spandex with a fineness of 7D was prepared by dry spinning.
[0035] Embodiment 13 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: The polybutylene adipate diol with a molecular weight of 1800, dicyclohexylmethane 4,4'-diisocyanate and toluene diisocyanate were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:1.5 and reacted at 62°C for 110 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender propylene diamine was added in an amount of 6 mol% of dicyclohexylmethane 4,4'-diisocyanate and toluene diisocyanate to obtain a mixed solution A with an isocyanate content of >10 mol% and a prepolymer content of 20 wt%; Then, wood pulp regenerated cellulose with a polymerization degree of 500 is dissolved in a DMAc solution of LiCl to form a mixed solution B; the mass fractions of wood pulp cellulose and LiCl are 13wt% and 5wt% respectively; The mixed solution A and B were mixed and reacted at a mass ratio of 6:1 for 90 minutes, and then 5wt% of antioxidant 1076, nanoparticle silica, light stabilizer 144, and flame retardant melamine cyanurate were added and aged. An integral spinning assembly was used with 100 spinnerets, 2 spinning winding heads, and a winding speed of 700m / min, and high-strength spandex with a fineness of 20D was prepared by dry spinning.
[0036] Embodiment 14 This embodiment provides a method for preparing high-strength spandex fiber, comprising the following steps: Polytetramethyleneimine with a molecular weight of 1500 and 1,5-naphthalene diisocyanate were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:2.1 and reacted at 52°C for 155 minutes to prepare an isocyanate-terminated prepolymer solution, and p-phenylenediamine, a chain extender, was added in an amount of 25 mol% of 1,5-naphthalene diisocyanate to obtain a mixed solution A with an isocyanate ratio of >10 mol% and a prepolymer ratio of 30 wt%; Then, bamboo pulp regenerated cellulose with a polymerization degree of 600 is dissolved in a DMAc solution of LiCl to form a mixed solution B, and the viscosity of the mixed solution B is 50 Pa.s; the mass fractions of wood pulp cellulose and LiCl are 13wt% and 11wt% respectively; The mixed solution A and B were mixed and reacted in a mass ratio of 1:1 for 60 minutes, and then 4.8wt% of antioxidant 168, nano-particle titanium dioxide, stabilizer zinc oxide, and flame retardant dimethyl methylphosphonate were added and aged. An integral spinning assembly was used with 120 spinnerets, 4 spinning winders, and a winding speed of 900m / min, and high-strength spandex with a fineness of 20D was prepared by dry spinning.
[0037] Comparative Example 1 This comparative example provides a method for preparing high-strength spandex fiber, which differs from Example 1 in that cellulose modification is not performed, and the steps are as follows: Polytetramethylene glycol with a molecular weight of 1000 and 1,5-naphthalene diisocyanate were dissolved in N,N-dimethylacetamide solution at a molar ratio of 1:1.6 and reacted at 75°C for 70 minutes to prepare an isocyanate-terminated prepolymer solution, and a chain extender propylene diamine was added in an amount of 8 mol% of 1,5-naphthalene diisocyanate to obtain a mixed solution with an isocyanate ratio of >10 mol% and a prepolymer ratio of 26wt%; Then, 0.1wt% of the total weight of antioxidant 1076, nano-particle titanium dioxide, light stabilizer 783, and flame retardant melamine cyanurate were added and then aged; an integral spinning assembly was used, the number of spinnerets was 60, the number of spinning winders was 3, and the winding speed was 1000m / min. Spandex with a fineness of 8D was prepared by dry spinning.
[0038] The breaking strength of the obtained 8D spandex fiber is 1.24 cN / detx, the breaking elongation is 568%, and the initial thermal decomposition temperature is 245°C.
[0039] The tensile properties and thermal decomposition properties of the high-strength spandex fibers prepared in Examples 1-14 are shown in Table 1: Table 1: As shown in Table 1, by copolymerizing cellulose with a certain degree of polymerization with a polyurethane prepolymer, the microphase separation degree of the molecular chain can be significantly improved and the rigidity and flexibility of the molecular chain can be regulated, thereby obtaining a spandex fiber with a mechanical strength greater than 1.5 cN / detx, an elongation at break that can be adjusted between 100-600%, and excellent thermal stability.
[0040] In the comparative example, the composition of conventional spandex molecules is that since the molecular chain does not contain cellulose structure, the degree of microphase separation of the molecular chain and the regulation of the rigidity and flexibility of the molecular chain are not improved. Therefore, its elongation at break is greater than 500%, the elasticity is relatively high, but the breaking strength is only 1.2 cN / dtex, and the thermal decomposition temperature is 245°C, and it does not have high strength and heat resistance.
[0041] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing high-strength spandex fiber, characterized in that: Here are the steps: (1) reacting a polydiol with a diisocyanate in an organic solvent to obtain an isocyanate-terminated prepolymer solution; then adding a chain extender to obtain a mixed solution A; (2) dissolving the regenerated cellulose in an organic solvent of LiCl to form a mixed solution B; (3) Mixing the mixed solution A and the mixed solution B for reaction, adding an auxiliary agent and then aging; High-strength spandex is prepared by dry spinning.
2. The method for preparing high-strength spandex fiber according to claim 1, characterized in that: In the step (1), the molar ratio of the polyglycol to the diisocyanate is 1:(1.5-2.5), the prepolymer accounts for 20-40wt% in the mixed solution A, the reaction conditions are 40-80°C, and the reaction time is 60-180min.
3. The method for preparing high-strength spandex fiber according to claim 1, characterized in that: The proportion of isocyanate in the terminal groups of the prepolymer in the mixed solution A is greater than 10 mol %, and the organic solvent in step (1) and step (2) is DMAc.
4. The method for preparing high-strength spandex fiber according to claim 1, characterized in that: The polyglycol in step (1) is a polyether polyol or polyester polyol with a molecular weight of 1000-3000; the polyether diol is polytetramethylene glycol, polyethylene glycol or polypropylene glycol; the polyester diol is polybutylene succinate diol, polybutylene adipate diol or polybutylene sebacate diol.
5. The method for preparing high-strength spandex fiber according to claim 1, characterized in that: The diisocyanate in step (1) is any one of 4,4'-methylenebis(phenyl isocyanate), 1,5-naphthalene diisocyanate, dicyclohexylmethane 4,4'-diisocyanate, toluene diisocyanate and 4,4'-diisocyanato-3,3'-dimethylbiphenyl.
6. The method for preparing high-strength spandex fiber according to claim 1, characterized in that: In the step (1), the chain extender is any one of ethylenediamine, propylenediamine, methylcyclohexanediamine, pentamethylenediamine and p-phenylenediamine, and the amount used is 5-25 mol% of the diisocyanate.
7. The method for preparing high-strength spandex fiber according to claim 1, characterized in that: In the mixed solution B in step (2), the regenerated cellulose is 1-20wt%; the LiCl is 5-12wt%; the polymerization degree of the regenerated cellulose is 200-600; the source of the regenerated cellulose is any one of wood pulp, bamboo pulp, mushroom grass, rice straw and wheat straw.
8. The method for preparing high-strength spandex fiber according to claim 1, characterized in that: In the step (3), the mass ratio of the mixed solution A to the mixed solution B is 1-20:1, and the mixing time is 30-90 min; the auxiliary agents are antioxidants, nanoparticles, stabilizers and flame retardants, and the total amount of the auxiliary agents is 0.1-5wt% of the total mass of the spinning solution.
9. The method for preparing high-strength spandex fiber according to claim 1, characterized in that: The method for preparing bio-based spandex fiber comprises the following steps: the dry spinning is an integral spinning assembly, the number of spinning holes is ≥60, the number of spinning winding heads is ≥2, and the winding speed is 600-1200 m / min.
10. The high-strength spandex fiber prepared by the method according to any one of claims 1 to 9, characterized in that: The high-strength spandex fiber has a fineness of ≥7D, a breaking strength of ≥1.5cN / detx, a breaking elongation of 100-600%, and a thermal decomposition temperature of ≥300°C.
Citation Information
Cited By
High-recovery spandex fiber and preparation method thereof
CN119409921A