Phosphate water reducing agent as well as preparation method and application thereof
The high molecular weight phosphate water reducer is prepared by reacting polyethylene polyamine with polyepoxy compounds, which solves the problems of small molecular weight and poor compatibility of existing phosphate water reducer, and achieves better concrete flow and resistance The clay performance improves the adaptability and stability of cement-based materials.
Patent Information
- Application Number
- CN202310511060.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-08
AI Technical Summary
The existing phosphate-based water reducing agent has a low molecular weight and limited spatial steric resistance, which leads to low water reduction rate and poor compatibility with cement and gravel, resulting in rapid slump loss and easy cracking of concrete.
By reacting polyethylene polyamine monomer with polyepoxy compounds, a long-chain or branched polyamine compound is obtained, and a substitution reaction is carried out with chlorinated polyether, followed by phosphorylation to prepare a high molecular weight phosphate salt Water reducing agent increases its molecular weight and steric hindrance, thereby improving its dispersion and clay resistance.
The obtained phosphate water reducing agent has strong adsorption ability and dispersion properties, which can effectively improve the adaptability and clay resistance of cement-based materials, improve the initial flow and slump retention of concrete, and reduce the risk of cracking.
Smart Images

Figure QLYQS_1 
Figure BDA0004217510130000031 
Figure BDA0004217510130000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete admixtures, and particularly relates to a phosphate water reducing agent, a preparation method and application thereof. Background Art
[0002] Concrete admixtures are substances added during the mixing process to improve the performance of concrete. According to their main functions, they can be divided into four categories: admixtures that improve the rheological properties of concrete mixtures, including various water reducers, air entraining agents and pumping agents; admixtures that adjust the setting time and hardening properties of concrete, including retarders, early strength agents and quick setting agents. Admixtures that improve the durability of concrete include air entraining agents, waterproofing agents and rust inhibitors; admixtures that improve other properties of concrete include air entraining agents, expansion agents, antifreeze agents, colorants, waterproofing agents and pumping agents. With the advancement of construction engineering technology, the addition of admixtures is no longer just to save raw materials, but has become the main measure to improve the performance of concrete. Water reducers account for more than 70% of all admixtures used, and are the most widely used and widely used type of concrete admixtures.
[0003] After decades of development, water reducers have evolved from the earliest lignin sulfonate common water reducers to high-efficiency water reducers represented by melamine and naphthalene series, and then to the widely used polycarboxylate high-performance water reducers with better performance. The comb-shaped molecular structure of polycarboxylate water reducers can increase the steric hindrance between particles after being adsorbed on cement particles, making its water reducing performance much better than other water reducers. However, with the advancement of engineering construction, high-quality sand and gravel resources for concrete are becoming increasingly scarce. Excessive development of river sand has caused a shortage of river sand. More and more projects use artificial sand and machine-made sand. At the same time, each construction site uses local materials, which results in that the sand and gravel aggregates in each project are often very different, and the mud content of sand and gravel aggregates in some areas is gradually increasing. In actual use, the performance of polycarboxylate water reducers is often affected by mixing factors such as cement composition and aggregates. The increasingly serious compatibility problem between water reducers and different types of cement sand and gravel has received widespread attention. Its compatibility problems are mainly manifested as: the water-reducing agent has no water-reducing effect, the newly mixed concrete has serious water bleeding and segregation phenomenon, the slump of concrete is lost very quickly, and abnormal coagulation occurs; the strength of hardened concrete at each age has no obvious increase, the concrete shrinkage increases, and it is easy to crack.
[0004] The phosphate group has a large electronegative property, a strong complexing ability with calcium ions, and a stronger adsorption capacity than the carboxyl group. For this reason, many researchers have introduced phosphate groups into water reducers to enhance the performance of water reducers. Patent CN202110083268.6 discloses a polycarboxylic acid water reducer with a polyphosphate ester side chain and a preparation method thereof. First, 2-chloro-oxy-1,3,2-dioxaphospholane and a monohydric alcohol are used to prepare an intermediate under the action of a catalyst, and then the intermediate is subjected to ring-opening polymerization with polyethylene glycol monomethyl ether to obtain a polyethylene glycol-polyphosphate ester monomethyl ether linear macromolecule, and finally the linear macromolecule is subjected to an esterification grafting reaction with polyacrylic acid to prepare a polycarboxylic acid water reducer with a polyphosphate ester side chain. The polycarboxylic acid water reducer with a polyphosphate ester side chain prepared by the invention has an amphiphilic property and provides a stronger steric hindrance effect, thereby obtaining a stronger dispersibility than a traditional polycarboxylic acid water reducer; the side chain can fundamentally inhibit the intercalation of the side chain in the soil, and has excellent anti-mud and plastic properties. Patent CN108084428B discloses a method for preparing a medium-low molecular weight phosphonic acid-based water reducer and its application. The initiator 3-chloro-1,2-propylene glycol is obtained by reacting epichlorohydrin with water, and then the initiator 3-chloro-1,2-propylene glycol is condensed with ethylene oxide to obtain a chlorinated polyether. The chlorinated polyether is then aminated and phosphitated to obtain a medium-low molecular weight phosphonic acid-based high-efficiency water reducer. The obtained medium-low molecular weight phosphonic acid-based water reducer has good adaptability to cement and admixtures as a cement-based material dispersant, good dispersion and slump retention performance, and excellent anti-clay performance. Patent CN201710119909.2 discloses a method for preparing a polycarboxylic acid water reducer containing a phosphoric acid group. First, a terminal ethylenically unsaturated phosphoric acid monomer is prepared, and then it is added to the synthesis of the polycarboxylic acid water reducer. This water reducer introduces terminal ethylenically unsaturated phosphoric acid monomers into the structure, which is beneficial to initial adsorption, improves initial dispersibility, delays cement hydration and agglomeration, effectively improves slump retention, reduces sensitivity to concrete, and enhances mud resistance and adaptability to different aggregates. Patent CN201510491861.9 discloses a polyphosphoric acid water reducer made from the following raw materials: a. methyl allyl polyoxyethylene ether; b. acrylic acid or methacrylic acid; c. vinyl phosphoric acid; d. ammonium persulfate; e. mercaptoacetic acid or mercaptopropionic acid; f. trisodium phosphate. Among them, the molar ratio of raw materials a, b, c, and f is: 1:3-4:0.2-1:2-3; raw material d is 0.2%-0.5% of the total weight of the material; raw material e is 0.1%-0.3% of the total weight of the material. In addition, the invention also discloses a method for synthesizing a polyphosphoric acid water reducer. The phosphoric acid and carboxylic acid copolymer water reducer of the present invention has better water reduction effect and slump retention effect than ordinary polycarboxylic acid water reducer, and has a certain retarding effect on concrete. Most of the above phosphate water reducers introduce unsaturated phosphate monomers into the synthesis of polycarboxylic acid water reducers to obtain polycarboxylic acid water reducers containing phosphoric acid groups through free radical polymerization, but unsaturated phosphoric acid monomers are difficult to prepare at this stage and do not meet the conditions for industrial production.Another part of water reducers whose adsorption groups are all phosphate groups generally have lower molecular weight and provide limited steric hindrance in cement adsorption, resulting in their water reduction rate not being very high. Summary of the invention
[0005] In order to solve the technical problems of low molecular weight and limited steric hindrance of phosphate-based water reducers in the prior art, the present invention provides a phosphate water reducer, a preparation method and its application. The phosphate water reducer is a water reducer with a long chain or branched all-phosphate adsorption group, with a large molecular weight, large steric hindrance, and strong phosphite adsorption capacity, so that the water reducer has strong dispersibility, good adaptability to cement adhesives, and good anti-clay performance.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A phosphate water reducer, wherein a polyethylene polyamine monomer is reacted with a polyepoxy compound to obtain a long-chain or branched polyamine compound, the polyamine compound is then subjected to a substitution reaction with a chlorinated polyether, and then the active hydrogen in the polyamine compound is subjected to a phosphitylation reaction with phosphorous acid to obtain the phosphate water reducer; the polyethylene polyamine monomer is ring-openedly connected to the epoxy group of the polyepoxy compound through an amine group, and the amine group of the polyamine compound is connected to the chlorinated polyether through a substitution reaction;
[0008] The molar ratio of the polyethylene polyamine monomer to the polyepoxy compound is 1:0.5-1;
[0009] The molar ratio of the chlorinated polyether to the polyethylene polyamine monomer is 1:0.5-2;
[0010] The molecular weight Mw of the phosphate water reducer is 10000-25000.
[0011] Further, the molar ratio of the phosphorous acid to the active hydrogen in the polyamine compound is 1:1-2;
[0012] Furthermore, the polyethylene polyamine monomer can be one or a mixture of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, and hexaethyleneheptamine.
[0013] Furthermore, the polyepoxy compound can be a mixture of one or more of diglycidyl ether, ethylene glycol diglycidyl ether, butanediol diglycidyl ether, bisphenol A diglycidyl ether, glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol glycidyl ether, and the like.
[0014] Furthermore, the chlorinated polyether has the following structural formula (I):
[0015]
[0016] Wherein, AO represents a repeating unit of chlorinated polyether, which is a mixture of ethylene oxide and propylene oxide; n is the average added mole number of AO, and n is an integer not greater than 200; (AO) n It is a homopolymer, random copolymer or block copolymer structure, and the molecular weight Mw of the chlorinated polyether is 500-5000.
[0017] On the other hand, the present invention also provides a method for preparing a phosphate water reducer, and the method for preparing the phosphate water reducer specifically comprises the following steps:
[0018] (1) Adding polyethylene polyamine monomers into a reaction vessel, and then adding a polyepoxy compound while controlling the temperature at 50-120° C., reacting for 0.5-3 hours, to obtain a long-chain or branched polyamine compound;
[0019] (2) adding water to step (1), then adding chlorinated polyether while controlling the temperature at 80-130° C., reacting for 3-6 hours, grafting the chlorinated polyether onto the polyamine compound, and obtaining a polyamine compound with a polyether chain;
[0020] (3) In step (2), an acid catalyst, phosphorous acid and formaldehyde are added to phosphite the product in step 2. After the reaction is completed and cooled, the product is neutralized with liquid alkali to a pH of 3-7 to obtain a phosphate water reducer.
[0021] Furthermore, the amount of water added in step (2) is 20%-40% by mass of the chlorinated polyether.
[0022] The reaction temperature in step (3) is 80-150° C., and the reaction time is 3-8 hours.
[0023] The acid catalyst in step (3) can be one of phosphoric acid, sulfuric acid, and p-toluenesulfonic acid, and the content of the acid catalyst is 3%-10% by weight of the reactants.
[0024] The molar ratio of formaldehyde to phosphorous acid in step (3) is 1:0.8-1.
[0025] The invention also provides application of the phosphate water reducer as a dispersant for cement-based materials.
[0026] The phosphate water reducer obtained by the present invention has good dispersibility as a cement-based material dispersant, good adaptability to cement and admixtures, and strong anti-clay performance. When used, its dosage (solid dosage) is 0.8‰-3.5‰ of the mass of the cementitious material, and the specific dosage is determined according to actual engineering needs.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The present invention obtains a linear or branched polyamine compound by reacting a polyamine with a polyepoxy compound, and the amine part of the polyamine compound is grafted with a chlorinated polyether, and a part of the phosphite reaction is performed to obtain the phosphate water reducer. The phosphate water reducer has a large molecular weight, and due to the strong adsorption capacity of the phosphate group, the water reducer has a strong adsorption capacity. In addition, the steric hindrance of the polyether chain, the obtained condensation-type phosphate water reducer has good dispersibility, anti-clay performance and adaptability to cement. Through the reaction of polyepoxy compounds and polyamines, the molecular weight of the water reducer can be increased, the steric hindrance of the water reducer can be increased, and thus the dispersibility of the phosphonate water reducer can be improved.
[0029] (2) The reaction conditions are simple and easy to operate, and the obtained water reducer has stable structure and performance, and the molecular weight can be controlled and adjusted.
[0030] (3) The phosphate water reducer provided by the present invention can be used alone or in combination with other water reducers on the market. DETAILED DESCRIPTION
[0031] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the examples, but the content of the present invention is not limited to the following examples. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0032] In the examples and comparative examples of the present invention, the molecular weight of the condensate was measured using a Wyatt Technology Corporation gel permeation chromatograph (GPC). The experimental conditions are as follows:
[0033] Gel column: Shodex SB806+803 two chromatographic columns connected in series;
[0034] Washing solution: 0.1M NaNO3 solution;
[0035] Mobile phase speed: 1.0 mL / min;
[0036] Injection: 20uL 0.5% aqueous solution;
[0037] Detector: Shodex RI-71 differential refractometer;
[0038] Standard: polyethylene glycol GPC standard (Sigma-Aldrich, molecular weight 1010000, 478000, 263000, 118000, 44700, 18600, 6690, 1960, 826, 232).
[0039] The structural parameters of the chlorinated polyethers in the embodiments and comparative examples are shown in Table 1 below:
[0040] Table 1 Names and structural parameters of chlorinated polyethers
[0041] Polyether Name Chlorinated polyether structural parameters Molecular weight Mw P1 The molar ratio of ethylene oxide to propylene oxide is 4:1, n=50 2418 P2 The molar ratio of ethylene oxide to propylene oxide is 50:0, n=50 2278 P3 The molar ratio of ethylene oxide to propylene oxide is 8:1, n=90 4178 P4 The molar ratio of ethylene oxide to propylene oxide is 4:1, n=50 2418 P5 The molar ratio of ethylene oxide to propylene oxide is 6:1, n=70 3298 P6 The molar ratio of ethylene oxide to propylene oxide is 1:1, n=60 3138 P7 The molar ratio of ethylene oxide to propylene oxide is 5:2, n=70 3438 P8 The molar ratio of ethylene oxide to propylene oxide is 10:0, n=10 518
[0042] Example 1
[0043] (1) Synthesis of polyamine compounds: After drying in an oven, a 500 mL three-necked flask with stirring was taken out, 10.3 g of diethylenetriamine was added, and after heating to 70°C, 13 g of diglycidyl ether was added dropwise. After the addition was completed, the reaction was continued for 2 hours to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 40 g of water and 107.4 g of chloropolyether P1 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 120°C for 4 hours to graft the polyether onto the polyamine compound. (3) Phosphite reaction: 8.5 g of sulfuric acid, 20.5 g of phosphorous acid, and 24.32 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 120°C for 5 hours. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 5, and phosphate water reducer S1 with a molecular weight of Mw = 13952 was obtained.
[0044] Example 2
[0045] (1) Synthesis of polyamine compounds: After drying in an oven, a 500 mL three-necked flask with stirring was taken out, 18.9 g of tetraethylene pentamine was added, and after heating to 80°C, 17.4 g of ethylene glycol diglycidyl ether was added dropwise. After the addition was completed, the reaction was continued for 2 h to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 70 g of water and 227.8 g of chloropolyether P2 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 120°C for 4 h to graft the polyether onto the polyamine compound. (3) Phosphation reaction: 10 g of sulfuric acid, 32.8 g of phosphorous acid, and 24.32 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 120°C for 5 h. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 5, and phosphate water reducer S1 was obtained, with a molecular weight Mw = 14596.
[0046] Example 3
[0047] (1) Synthesis of polyamine compounds: After drying in an oven, a 1000 mL three-necked flask with stirring was taken out, and 23.2 g of pentaethylene hexamine was added. After heating to 90°C, 20.2 g of butanediol diglycidyl ether was added dropwise. After the addition was completed, the reaction was continued for 2 hours to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 130 g of water and 417.8 g of chloropolyether P3 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 80°C for 6 hours to graft the polyether onto the polyamine compound. (3) Phosphation reaction: 30 g of phosphoric acid, 27.33 g of phosphorous acid, and 30.03 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 80°C for 8 hours. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 3, and the phosphate water reducer S3 with a molecular weight of Mw = 21975 was obtained.
[0048] Example 4
[0049] (1) Synthesis of polyamine compounds: After drying in an oven, a 1000 mL three-necked flask with stirring was taken out, 27.5 g of hexaethylene heptamine was added, and after heating to 100°C, 34 g of bisphenol A diglycidyl ether was added dropwise. After the addition was completed, the reaction was continued for 1 hour to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 130 g of water and 483.6 g of chloropolyether P4 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 120°C for 4 hours to graft the polyether onto the polyamine compound. (3) Phosphite reaction: 25 g of phosphoric acid, 20.5 g of phosphorous acid, and 20.27 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 110°C for 5 hours. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 6, and phosphate water reducer S4 was obtained, with a molecular weight Mw=18564.
[0050] Example 5
[0051] (1) Synthesis of polyamine compounds: After drying in an oven, a 1000 mL three-necked flask with stirring was taken out, and 5.15 g of diethylenetriamine and 13.75 g of hexaethyleneheptamine were added. After heating to 110°C, 26 g of propylene glycol triglycidyl ether was added dropwise. After the addition was completed, the reaction was continued for 0.5 h to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 160 g of water and 329.8 g of chloropolyether P5 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 110°C for 4 h to graft the polyether onto the polyamine compound. (3) Phosphation reaction: 40 g of phosphoric acid, 24.6 g of phosphorous acid, and 30.41 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 120°C for 4 h. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 7, and the phosphate water reducer S5 with a molecular weight of Mw = 23925 was obtained.
[0052] Example 6
[0053] (1) Synthesis of polyamine compounds: After drying in an oven, a 1000 mL three-necked flask with stirring was taken out, and 6.0 g of ethylenediamine and 11.6 g of tetraethylenepentamine were added. After heating to 120°C, 20.8 g of propylene glycol triglycidyl ether was added dropwise. After the addition was completed, the reaction was continued for 0.5 h to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 150 g of water and 313.8 g of chloropolyether P6 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 120°C for 3 h to graft the polyether onto the polyamine compound. (3) Phosphation reaction: 35 g of p-toluenesulfonic acid, 17.22 g of phosphorous acid, and 21.28 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 100°C for 5 h. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 5, thereby obtaining a phosphate water reducer S6 with a molecular weight Mw=21597.
[0054] Example 7
[0055] (1) Synthesis of polyamine compounds: After drying in an oven, a 500 mL three-necked flask with stirring was taken out, and 5.15 g of diethylenetriamine and 7.3 g of triethylenetetramine were added. After heating to 50°C, 18.08 g of propylene glycol triglycidyl ether was added dropwise. After the addition was completed, the reaction was continued for 3 hours to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 86 g of water and 171.9 g of chloropolyether P7 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 130°C for 5 hours to graft the polyether onto the polyamine compound. (3) Phosphation reaction: 17 g of sulfuric acid, 21.32 g of phosphorous acid, and 23.42 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 110°C for 5 hours. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 5, and the phosphate water reducer S7 with a molecular weight of Mw = 19347 was obtained.
[0056] Example 8
[0057] (1) Synthesis of polyamine compounds: After drying in an oven, a 500 mL three-necked flask with stirring was taken out, and 3.0 g of ethylenediamine and 13.75 g of hexaethylene heptamine were added. After heating to 60°C, 18 g of pentaerythritol glycidyl ether was added dropwise. After the addition was completed, the reaction was continued for 0.5 h to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 40 g of water and 51.8 g of chloropolyether P8 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 90°C for 6 h to graft the polyether onto the polyamine compound. (3) Phosphation reaction: 4.0 g of phosphoric acid, 24.6 g of phosphorous acid, and 27.03 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 90°C for 6 h. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 5, and the phosphate water reducer S8 with a molecular weight of Mw = 11569 was obtained.
[0058] Example 9
[0059] (1) Synthesis of polyamine compounds: After drying in an oven, a stirred 500 mL three-necked flask was taken out, and 7.3 g of triethylenetetramine and 9.45 g of tetraethylenepentamine were added. After heating to 70°C, 4.55 g of diglycidyl ether and 9.1 g of propylene glycol triglycidyl ether were added dropwise. After the addition was complete, the reaction was continued for 2 h to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 40 g of water and 107.4 g of chloropolyether P1 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 100°C for 4 h to graft the polyether onto the polyamine compound. (3) Phosphation reaction: 8.5 g of sulfuric acid, 30.75 g of phosphorous acid, and 38.01 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 140°C for 3 h. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 5, thereby obtaining a phosphate water reducer S9 with a molecular weight of Mw = 15315.
[0060] Example 10
[0061] (1) Synthesis of polyamine compounds: After drying in an oven, a stirred 500 mL three-necked flask was taken out, and 9.45 g of tetraethylene pentamine and 11.6 g of pentaethylene hexamine were added. After heating to 80°C, 4.55 g of diglycidyl ether and 12.6 g of pentaerythritol glycidyl ether were added dropwise. After the addition was complete, the reaction was continued for 2 h to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 113 g of water and 227.8 g of chloropolyether P2 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 110°C for 4 h to graft the polyether onto the polyamine compound. (3) Phosphite reaction: 18.8 g of phosphoric acid, 36.08 g of phosphorous acid, and 44.59 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 140°C for 3 h. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 5, thereby obtaining a phosphate water reducer S10 with a molecular weight Mw=18612.
[0062] Embodiment 11
[0063] (1) Synthesis of polyamine compounds: After drying in an oven, a 500 mL three-necked flask with stirring was taken out, and 5.15 g of diethylenetriamine and 11.6 g of pentaethylenehexamine were added. After heating to 90°C, 6.96 g of ethylene glycol diglycidyl ether and 10.4 g of propylene glycol triglycidyl ether were added dropwise. After the addition was complete, the reaction was continued for 2 h to obtain a polyamine compound. (2) Synthesis of polyamine compounds with polyether chains: 40 g of water and 107.4 g of chloropolyether P1 were added to the reaction flask of the synthesized polyamine compound, and the reaction was carried out at 110°C for 4 h to graft the polyether onto the polyamine compound. (3) Phosphation reaction: 7.2 g of sulfuric acid, 28.7 g of phosphorous acid, and 35.47 g of formaldehyde were added to the reaction flask, and the reaction was carried out at 150°C for 5 h. After the reaction, the temperature was lowered to room temperature, and the pH was neutralized with liquid alkali to 5, thereby obtaining a phosphate water reducer S11 with a molecular weight Mw=14351.
[0064] Comparative Example 1
[0065] According to the method in Example 1 of patent CN108084428B, a medium-low molecular weight phosphonic acid-based water reducer was prepared, denoted as S12, with a molecular weight of Mw=3524.
[0066] Comparative Example 2
[0067] In a 500mL three-necked flask with stirring, 10.3g of diethylenetriamine, 40g of water, and 107.4g of chlorinated polyether P1 were added, and the mixture was reacted at 120°C for 4h to graft the polyether onto the polyamine compound. (3) Phosphation reaction: 8.5g of sulfuric acid, 20.5g of phosphorous acid, and 24.32g of formaldehyde were added to the reaction flask, and the mixture was reacted at 120°C for 5h. After the reaction, the mixture was cooled to room temperature and neutralized with liquid alkali to a pH of 5 to obtain phosphate water reducer S13 with a molecular weight of Mw = 3258.
[0068] Application Example 1
[0069] The cement paste fluidity test was carried out according to GB / T8077-2000 standard, with 87g of water added and the cement paste fluidity was measured on a flat glass after stirring for 3 minutes. The cements used were Onoda 42.5RP‖, Helin 42.5RPO, Conch 42.5RPO, and benchmark cement PⅠ42.5 to test the cement paste fluidity. The results are shown in Table 1 below.
[0070] Table 1 Cement paste fluidity evaluation table
[0071]
[0072] The slurry test was carried out using Onoda, Helin, Conch and benchmark cements. It can be seen from Table 1 that the phosphate-based high-efficiency water reducer prepared by the present invention has good dispersibility when the dosage is 0.09%, good adaptability to cement, large initial fluidity, and small fluidity loss after 1 hour, and good slump retention. However, S-12 and S-13 have poor dispersibility due to their small molecular weight. The main reason why the synthesized water reducer has better dispersibility is that after the introduction of the phosphate adsorption group, the Ca 2+ The complexing effect is enhanced, thereby enhancing the adaptability of phosphate-based water reducer to cement, and the retarding effect of phosphate group makes the water reducer have better slump retention performance. The introduction of polyepoxide compounds into cross-linking makes the molecular weight of the obtained water reducer larger, provides greater steric hindrance, and has better dispersibility of the water reducer.
[0073] Anti-clay mortar experiments were carried out on S-1, S-12 and S13. 750g cement, 1350g standard sand and 247.5g water were used, and montmorillonite with different cement masses was added respectively. The results are shown in Table 2. It can be seen that after adding montmorillonite, the initial fluidity and 30min fluidity of cement mortar decreased, and the dispersibility and slump retention of water reducer decreased. However, the dispersibility of S-1 was better than that of S-12 and S-13, and the slump retention was also better. Even with 1.5% montmorillonite, the phosphate-based water reducer could flow about 190mm, while the low molecular weight phosphate-based water reducers S-12 and S-13 basically did not flow, indicating that the synthesized high molecular weight phosphate-based water reducer has better anti-clay performance.
[0074] Table 2 Comparison of the fluidity of the slurry with different montmorillonite content
[0075]
[0076] Application Example 2
[0077] Referring to the test requirements of high-performance water reducing agent in the national standard GB8076-2008 "Concrete Admixture", the cement used is Onoda 525.5RPⅡ cement, the sand is medium sand with a fineness modulus Mx=2.6, and the gravel is a continuously graded crushed stone with a particle size of 5-10mm and a particle size of 10-20mm. The air content, slump, expansion and collapse retention performance of the polycondensate water reducing agent are tested according to the ratio specified in Table 3. The additive dosage is the solid dosage, and the test results are shown in Table 4. The dosage of the embodiment is 0.13%.
[0078] Table 3 Test concrete mix ratio
[0079]
[0080] Table 4 Concrete performance evaluation table
[0081]
[0082] The concrete fluidity data in Table 4 show that at 0.5% montmorillonite content, the phosphate-based water reducer exhibits better initial dispersibility and slump retention of concrete, while the low molecular weight phosphonic acid-based water reducers S-12 and S-13 have worse dispersibility and slump retention. This indicates that the synthesized high molecular weight phosphate water reducer has good anti-clay performance.
Claims
1. A phosphate water reducer, characterized in that: The phosphate water reducer is obtained by reacting a polyethylene polyamine monomer with a polyepoxy compound to obtain a long-chain or branched polyamine compound, and then the polyamine compound undergoes a substitution reaction with a chlorinated polyether, and then the active hydrogen in the polyamine compound undergoes a phosphitylation reaction with phosphorous acid to obtain the phosphate water reducer; the polyethylene polyamine monomer is ring-openedly connected with the epoxy group of the polyepoxy compound through an amine group, and the amine group of the polyamine compound is connected with the chlorinated polyether through a substitution reaction; The molar ratio of the polyethylene polyamine monomer to the polyepoxy compound is 1:0.5-1; The molar ratio of the chlorinated polyether to the polyethylene polyamine monomer is 1:0.5-2.
2. The phosphate water reducer according to claim 1, characterized in that: The molecular weight Mw of the phosphate water reducer is 10000-25000.
3. The phosphate water reducer according to claim 1, characterized in that: The molar ratio of the phosphorous acid to the active hydrogen in the polyamine compound is 1:1-2.
4. The phosphate water reducer according to claim 1, characterized in that: The polyethylene polyamine monomer is one or a mixture of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine and hexaethyleneheptamine.
5. The phosphate water reducer according to claim 1, characterized in that: The polyepoxy compound is a mixture of one or more of diglycidyl ether, ethylene glycol diglycidyl ether, butanediol diglycidyl ether, bisphenol A diglycidyl ether, glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol glycidyl ether.
6. The phosphate water reducer according to claim 1, characterized in that: The chlorinated polyether has the following structural formula (I): Wherein, AO represents a repeating unit of chlorinated polyether, which is a mixture of ethylene oxide and propylene oxide; n is the average added mole number of AO, and n is an integer not greater than 200; (AO) n It is a homopolymer, random copolymer or block copolymer structure, and the molecular weight Mw of the chlorinated polyether is 500-5000.
7. The method for preparing the phosphate water reducer according to any one of claims 1 to 6, characterized in that: The specific steps include: (1) Adding polyethylene polyamine monomers into a reaction vessel, then controlling the temperature at 50-120° C., adding a polyepoxy compound, and reacting for 0.5-3 hours to obtain a long-chain or branched polyamine compound; (2) adding water to step (1), then controlling the temperature at 80-130° C., adding chlorinated polyether, and reacting for 3-6 hours to graft the chlorinated polyether onto the polyamine compound to obtain a polyamine compound with a polyether chain; (3) In step (2), an acid catalyst, phosphorous acid and formaldehyde are added to phosphite the product in step 2. After the reaction is completed and cooled, the product is neutralized with liquid alkali to a pH of 3-7 to obtain a phosphate water reducer.
8. The preparation method according to claim 7, characterized in that: The reaction temperature in step (3) is 80-150° C., and the reaction time is 3-8 hours.
9. The preparation method according to claim 7, characterized in that: The acid catalyst in step (3) is one of phosphoric acid, sulfuric acid and p-toluenesulfonic acid, and the content of the acid catalyst is 3%-10% by weight of the reactants.
10. The preparation method according to claim 7, characterized in that: The molar ratio of formaldehyde to phosphorous acid in step (3) is 1:0.8-1.