Core-shell type wollastonite-polypyrrole conductive composite material as well as preparation method and application thereof
By forming a core-shell wollastonite-polypyrrole conductive composite material on the surface of wollastonite, the problems of high cost and insufficient stability of high-performance conductive materials are solved, and high conductivity and chemical stability are achieved. Combined, suitable for the fields of conductive coatings and engineering plastics.
Patent Information
- Application Number
- CN202411331969.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-08
AI Technical Summary
High-performance conductive materials are costly and degraded in extreme environments, which limits their wide application, especially the problems of material stability and conductivity.
By mixing wollastonite with water and modifying it, and polymerizing it with pyrrole monomer and oxidizing agent, a core-shell wollastonite-polypyrrole conductive composite material is formed, and a chemical oxidation polymerization method is used to form on the surface of the modified wollastonite. Polypyrrole shell, improving electrical conductivity and chemical stability.
It achieves a combination of high conductivity and high stability, reduces production costs, is suitable for conductive coatings and conductive engineering plastics with no special requirements for color, and extends the service life of the material.
Smart Images

Figure BDA0005058884520000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of conductive composite materials, and in particular to a core-shell type wollastonite-polypyrrole conductive composite material and a preparation method and application thereof. Background Art
[0002] Wollastonite is a single-chain silicate mineral, the main component of which is Ca 3 Si 3 O 9 , triclinic system, usually in the form of flakes, radials or fibers, white with a slight gray tint, hardness 4.5-5.0. Due to its chemical stability and physical properties, wollastonite is often used as a filler or thickener for coatings, plastics and other products. Adding wollastonite to coatings can not only improve the hardness, wear resistance and corrosion resistance of the coating, but also reduce costs, which has certain economic benefits.
[0003] At present, conductive composite materials have a wide range of applications, including conductive plastics, conductive coatings, and conductive additives for lithium-ion batteries and supercapacitors. However, high-performance conductive materials often have high production costs, and performance degradation may occur after long-term use or in extreme environments, especially material stability and conductivity, which limits their widespread application. Summary of the invention
[0004] The object of the present invention is to provide a core-shell wollastonite-polypyrrole conductive composite material and a preparation method and application thereof, wherein the chemical stability and conductive performance of the composite material are improved.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a core-shell type wollastonite-polypyrrole conductive composite material, comprising the following steps:
[0007] mixing wollastonite with water to obtain a wollastonite suspension;
[0008] The wollastonite suspension is mixed with a modifier to perform modification to obtain modified wollastonite;
[0009] The modified wollastonite, pyrrole monomer, water and oxidant are mixed and polymerized to obtain a core-shell type wollastonite-polypyrrole conductive composite material.
[0010] Preferably, the mesh size of the wollastonite is 1000-1250 meshes, and the solid content of the wollastonite suspension is 40-60 wt %.
[0011] Preferably, the modifier includes one or more of vinyltriethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, 3-chloropropyltriethoxysilane, and 3-mercaptopropyltriethoxysilane.
[0012] Preferably, the mass ratio of the wollastonite to the modifier is (10-15):(3-7.5).
[0013] Preferably, the modification temperature is 70-90° C., the stirring speed is 600 r / min, and the time is 30-50 min.
[0014] Preferably, the mass ratio of the wollastonite to the pyrrole monomer is (10-15):(20-30).
[0015] Preferably, the oxidant includes one or more of hydrogen peroxide, ammonium persulfate, potassium persulfate, and ferric chloride, the mass fraction of the hydrogen peroxide is 30%, and the mass ratio of the oxidant to the wollastonite is (10-30):(10-15).
[0016] Preferably, the polymerization reaction temperature is 0-5°C and the time is 3-5h.
[0017] The invention provides a core-shell type wollastonite-polypyrrole conductive composite material prepared by the preparation method, wherein the modified wollastonite is used as the core and the polypyrrole is used as the shell.
[0018] The present invention also provides application of the core-shell wollastonite-polypyrrole conductive composite material in the field of conductive engineering plastics.
[0019] Beneficial effects of the present invention:
[0020] In the process of preparing the conductive composite material, the present invention modifies wollastonite and then forms a polypyrrole shell layer on the surface of the modified wollastonite by chemical oxidation polymerization, thereby giving the composite material conductive properties. On the one hand, wollastonite as a filler can improve the mechanical strength and wear resistance of the composite material; on the other hand, polypyrrole as a conductive polymer material can significantly improve the conductive properties of wollastonite powder and meet the needs of high conductivity applications.
[0021] The core-shell type wollastonite-polypyrrole conductive composite material prepared by the present invention has a core-shell structure with modified wollastonite as the core and polypyrrole as the shell. The core-shell structure allows polypyrrole to form a uniform coating layer on the surface of wollastonite. This uniform layered structure helps more efficient charge transfer, thereby improving the conductivity of the overall composite material; at the same time, the coating layer of polypyrrole can protect the wollastonite core from erosion by environmental factors (such as moisture, acid and alkali, etc.), reduce the occurrence of chemical reactions, and thus improve the chemical stability of the material. The present invention combines materials with high conductivity and high stability through the core-shell structure to obtain a composite material with both excellent conductive properties and chemical stability.
[0022] In addition, since the composite material prepared by the present invention is a black powder, it is only suitable for conductive coatings, conductive engineering plastics and other fields that have no special requirements on color, and is not applicable to other fields that have requirements on color; at the same time, wollastonite and polypyrrole are relatively easy to obtain as raw materials, which is conducive to reducing production costs and expanding the application field of wollastonite coatings to a certain extent. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing a core-shell type wollastonite-polypyrrole conductive composite material, comprising the following steps:
[0024] mixing wollastonite with water to obtain a wollastonite suspension;
[0025] The wollastonite suspension is mixed with a modifier to perform modification to obtain modified wollastonite;
[0026] The modified wollastonite, pyrrole monomer, water and oxidant are mixed and polymerized to obtain a core-shell type wollastonite-polypyrrole conductive composite material.
[0027] In the present invention, wollastonite is preferably mixed with water and ultrasonically dispersed to obtain a wollastonite suspension.
[0028] In the present invention, the mesh size of the wollastonite is preferably 1000-1250 meshes, and more preferably 1000-1200 meshes; the ultrasonic dispersion time is preferably 30 minutes; the solid content of the wollastonite suspension is preferably 40-60%, and more preferably 40-50%, and more preferably 40-45%; high-mesh wollastonite has a larger specific surface area, which is conducive to more wollastonite surfaces contacting with pyrrole monomers to form a more uniform core-shell structure, while effectively reducing agglomeration and improving the uniformity and stability of the material.
[0029] In the present invention, the wollastonite suspension is preferably mixed with a modifier to perform modification to obtain modified wollastonite.
[0030] In the present invention, the modifier preferably includes one or more of vinyl triethoxysilane, 3-glycidyloxypropyl methyl diethoxy silane, 3-chloropropyl triethoxy silane, and 3-mercaptopropyl triethoxy silane, and further preferably includes one or more of 3-glycidyloxypropyl methyl diethoxy silane and 3-mercaptopropyl triethoxy silane; the mass ratio of the wollastonite to the modifier is preferably (10-15):(3-7.5), further preferably (10-15):(3-6), and more preferably (10-15):(3-4.8); the modification of wollastonite can improve the surface properties of wollastonite and enhance the adhesion and compatibility between wollastonite and polypyrrole.
[0031] In the present invention, the modification temperature is preferably 70 to 90° C., more preferably 80 to 90° C., the stirring speed is preferably 600 r / min, and the time is preferably 30 to 50 min, more preferably 30 to 40 min.
[0032] After the modification is completed, the present invention preferably uses anhydrous ethanol and deionized water to repeatedly wash and centrifuge the product, places it in an electric heated blast drying oven, dries it at 60° C. for 24 hours, and grinds it to obtain modified wollastonite; the rotation speed during the centrifugation is preferably 3000 r / min.
[0033] In the present invention, the modified wollastonite, pyrrole monomer, water and an oxidant are preferably mixed to carry out a polymerization reaction to obtain a core-shell type wollastonite-polypyrrole conductive composite material.
[0034] In the present invention, the mass ratio of the wollastonite to the pyrrole monomer is preferably (10-15):(20-30), and more preferably (10-15):(20-25); the oxidant preferably includes one or more of hydrogen peroxide, ammonium persulfate, potassium persulfate, and trivalent iron ions, and more preferably includes one or more of hydrogen peroxide and ammonium persulfate. The mass fraction of hydrogen peroxide is preferably 30%. The mass ratio of the oxidant to the wollastonite is preferably (10-30):(10-15), and more preferably (10-20):(10-15), and more preferably (10-15):(10-15).
[0035] In the present invention, the polymerization reaction temperature is preferably 0 to 5° C., more preferably 0 to 3° C., and the polymerization reaction time is preferably 3 to 5 hours, more preferably 4 to 5 hours.
[0036] After the polymerization reaction is completed, the present invention preferably transfers the product to a centrifuge tube, centrifuges it in a centrifuge, washes it with anhydrous ethanol and deionized water, and finally dries it in a 60°C electric heated blast drying oven for 24 hours to obtain a core-shell type wollastonite-polypyrrole conductive composite material; the speed of the centrifuge is preferably 3000 r / min, and the time is preferably 5 min.
[0037] The invention provides a core-shell type wollastonite-polypyrrole conductive composite material prepared by the preparation method, wherein the modified wollastonite is used as the core and the polypyrrole is used as the shell.
[0038] The present invention also provides application of the core-shell wollastonite-polypyrrole conductive composite material in the field of conductive engineering plastics.
[0039] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0040] Example 1
[0041] 10 g of 1000 mesh wollastonite was mixed with 20 mL of water and ultrasonically dispersed for 30 min to obtain a wollastonite suspension;
[0042] The wollastonite suspension was mixed with 3 g of 3-glycidyloxypropylmethyldiethoxysilane, and modified at 80°C and 600 r / min. After 40 min, the mixture in the beaker was poured into a centrifuge tube, centrifuged and washed at 3000 r / min, and finally transferred to a 60°C electric heating blast drying oven for drying for 24 h to obtain modified wollastonite.
[0043] The modified wollastonite, 20 g of pyrrole monomer, 100 mL of water and 10 g of 30% hydrogen peroxide were mixed, and a polymerization reaction was carried out in an ice water bath at 3°C. After the reaction for 5 hours, the product was transferred to a centrifuge tube, washed several times with anhydrous ethanol and deionized water, and finally dried in an electric blast drying oven at 60°C for 24 hours to obtain the core-shell wollastonite-polypyrrole conductive composite material of Example 1.
[0044] Example 2
[0045] The only difference from Example 1 is:
[0046] The mass of wollastonite is 12 g;
[0047] The mass of pyrrole monomer is 25 g;
[0048] The oxidant is 30 g of ammonium persulfate;
[0049] The core-shell wollastonite-polypyrrole conductive composite material of Example 2 was obtained.
[0050] Example 3
[0051] The only difference from Example 1 is:
[0052] The mesh number of wollastonite is 1250 mesh and the mass is 12g;
[0053] The modifier is 3-mercaptopropyltriethoxysilane, with a mass of 4.8 g;
[0054] The mass of pyrrole monomer is 25 g;
[0055] The oxidant is 15g hydrogen peroxide;
[0056] The core-shell wollastonite-polypyrrole conductive composite material of Example 3 was obtained.
[0057] Example 4
[0058] The only difference from Example 1 is:
[0059] The mass of wollastonite is 15 g, and wollastonite is added to 30 mL of water;
[0060] The mass of the modifier is 6 g;
[0061] The mass of pyrrole monomer is 30 g;
[0062] The oxidant is 15g hydrogen peroxide;
[0063] The core-shell wollastonite-polypyrrole conductive composite material of Example 4 was obtained.
[0064] Example 5
[0065] The only difference from Example 1 is:
[0066] The mesh number of wollastonite is 1250 mesh, the mass is 15g, and the wollastonite is added into 30mL water; the modifier is 3-mercaptopropyltriethoxysilane, the mass is 7.5g;
[0067] The mass of pyrrole monomer is 30 g;
[0068] The oxidant is 30 g of ammonium persulfate;
[0069] The core-shell wollastonite-polypyrrole conductive composite material of Example 5 was obtained.
[0070] Comparative Example 1
[0071] The only difference from Example 1 is that the modifier is 3-mercaptopropyltriethoxysilane.
[0072] Comparative Example 2
[0073] The only difference from Example 1 is that the mass of the modifier is 4 g.
[0074] Comparative Example 3
[0075] The only difference from Example 1 is that the modification temperature is 90°C.
[0076] Basic characterization and conductivity test of composite materials:
[0077] The specific surface area of core-shell wollastonite-polypyrrole conductive composites was determined by BET method.
[0078] The particle size of the core-shell wollastonite-polypyrrole conductive composite material was measured by a laser particle size analyzer.
[0079] The core-shell wollastonite-polypyrrole conductive composite material was pressed into blocks by a powder tablet press, and its conductivity was measured by a ST2722-SZ four-probe resistance meter.
[0080] The test results of the examples are recorded in Table 1.
[0081] Table 1 Test results of conductive composite materials of Examples 1 to 5 and Comparative Examples 1 to 3
[0082]
[0083] Combining Example 1 and Comparative Examples 1 to 2, it can be seen that the modification effect of 3-glycidyloxypropylmethyldiethoxysilane on wollastonite is better than that of 3-mercaptopropyltriethoxysilane, which enables the subsequent polypyrrole shell layer to be better formed on the modified wollastonite surface, and when the mass ratio of polypyrrole to wollastonite increases, the polypyrrole shell layer becomes thicker, and the surface conductivity of the core-shell wollastonite-polypyrrole conductive composite material will also increase.
[0084] Combining Example 1 and Comparative Example 3, it can be seen that when a modifier is added to modify wollastonite, the optimal modification temperature is 80°C. When the temperature is higher than this optimal temperature, the modification effect of wollastonite decreases, resulting in unsatisfactory subsequent coating of polypyrrole, which reduces the surface conductivity of the wollastonite-polypyrrole conductive composite material.
[0085] It can be seen from Examples 1 to 5 and Comparative Examples 1 to 3 that the present invention provides a core-shell wollastonite-polypyrrole conductive composite material with modified wollastonite as the core and polypyrrole as the shell, which has good conductive properties and can be used in conductive coatings, conductive engineering plastics and other fields that have no requirements on color.
[0086] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a core-shell wollastonite-polypyrrole conductive composite material, characterized in that: The following steps are involved: mixing wollastonite with water to obtain a wollastonite suspension; The wollastonite suspension is mixed with a modifier to perform modification to obtain modified wollastonite; The modified wollastonite, pyrrole monomer, water and oxidant are mixed and polymerized to obtain a core-shell type wollastonite-polypyrrole conductive composite material.
2. The preparation method according to claim 1, characterized in that: The mesh number of the wollastonite is 1000-1250 meshes, and the solid content of the wollastonite suspension is 40-60wt%.
3. The preparation method according to claim 1, characterized in that: The modifier includes one or more of vinyl triethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, 3-chloropropyl triethoxysilane, and 3-mercaptopropyl triethoxysilane.
4. The preparation method according to claim 1 or 3, characterized in that: The mass ratio of the wollastonite to the modifier is (10-15):(3-7.5).
5. The preparation method according to claim 1, characterized in that: The modification temperature is 70-90° C., the stirring speed is 600 r / min, and the time is 30-50 min.
6. The preparation method according to claim 1, characterized in that: The mass ratio of the wollastonite to the pyrrole monomer is (10-15):(20-30).
7. The preparation method according to claim 1, characterized in that: The oxidant includes one or more of hydrogen peroxide, ammonium persulfate, potassium persulfate, and ferric chloride. The mass fraction of the hydrogen peroxide is 30%. The mass ratio of the oxidant to the wollastonite is (10-30):(10-15).
8. The preparation method according to claim 1, characterized in that: The polymerization reaction temperature is 0-5°C and the reaction time is 3-5h.
9. The core-shell wollastonite-polypyrrole conductive composite material prepared by the preparation method according to any one of claims 1 to 8, characterized in that: Modified wollastonite is used as the core and polypyrrole is used as the shell.
10. Use of the core-shell wollastonite-polypyrrole conductive composite material according to claim 9 in the field of conductive engineering plastics.