Aromatic polyimide powder for molded article, molded article using same, and method for improving mechanical strength of molded article

By adjusting the volatile components and process optimization in the aromatic polyimide powder, the problem of difficult to take into account both solvent resistance and mechanical characteristics in the prior art is solved, and the mechanical strength of the aromatic polyimide molded body is improved. and solvent resistance.

CN118909251APending Publication Date: 2024-11-08UBE CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411165079.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-03-13
Filing Date
2021-03-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, after using soluble polyimide or introducing fluorine functional groups, the solvent resistance and mechanical properties of the aromatic polyimide powder are difficult to fully demonstrate, and the solvent resistance of the molded body is easily damaged.

Method used

The amount of volatile components in the aromatic polyimide powder is adjusted to 0.50% to 5.00% by mass to ensure excellent mechanical characteristics of the molded body, and the powder characteristics are further optimized through the cleaning and drying process.

Benefits of technology

The mechanical strength of the aromatic polyimide molded body is achieved without damaging solvent resistance and significantly improving the mechanical strength of the aromatic polyimide molded body, providing a manufacturing method that can maximize the characteristics of the polyimide powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007620000000051
    Figure BDA0005007620000000051
  • Figure BDA0005007620000000061
    Figure BDA0005007620000000061
  • Figure BDA0005007620000000071
    Figure BDA0005007620000000071
Patent Text Reader

Abstract

Provided are: an aromatic polyimide powder for a molded article; a molded article using the aromatic polyimide powder; and a method for improving the mechanical strength of the molded article. Wherein the content of volatile components contained in the aromatic polyimide powder for molded bodies is 0.50-5.00% by mass with respect to 100% by mass of the aromatic polyimide powder at 25 DEG C, and the bending strength of the aromatic polyimide molded body obtained by molding is 60 MPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The application number of the original application is 202180019761.X, the application date is March 11, 2021, and the name of the invention is "Aromatic polyimide powder for molded bodies, molded bodies using the powder, and method for improving the mechanical strength of molded bodies." Technical Field

[0002] The present invention relates to a polyimide powder for a molded article having improved mechanical properties of the molded article, a molded article using the powder, and a method for improving the mechanical strength of the molded article. Background Art

[0003] Aromatic polyimides obtained from aromatic tetracarboxylic acid components and aromatic diamine components as main raw materials have excellent properties such as heat resistance, mechanical strength, electrical properties, and solvent resistance, and are widely used as materials for electrical and electronic parts, etc. Among them, aromatic polyimide powders processed into powder form can be filled into a mold and pressed to obtain a desired molded body, so they are widely used as materials for manufacturing parts for industrial manufacturing equipment.

[0004] In recent years, while effectively utilizing the characteristics of aromatic polyimide powders, the high functionality of aromatic polyimide powders has been actively carried out with the goal of further expanding the scope of application. For example, a method of mixing polyimide powders with various materials has been developed. Patent document 1 discloses a method of mixing polyimide powders and conductive carbon to obtain a molded body of an electric electronic component. In addition, patent document 2 discloses a method of mixing polyimide powders, inorganic fibrous fillers and solid lubricants to impart wear resistance and mechanical strength. In addition, patent document 3 discloses a method of mixing polyimide powders and fluorine-containing resin powders to improve the handling properties of polyimide powders.

[0005] However, when the polyimide powder is mixed with other additives or resins other than the polyimide powder, the content of the polyimide powder is relatively reduced, and as a result, the original properties of the polyimide powder cannot be fully exhibited.

[0006] In order to solve this problem, a method of chemically modifying polyimide powder is being adopted. For example, Patent Document 4 discloses the use of soluble polyimide. In addition, Patent Document 5 discloses a method of containing a fluorine functional group such as 2-hydroxy-1,1,1,3,3,3-hexafluoroisopropyl.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2007-016222

[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 62-0132960

[0011] Patent Document 3: International Publication No. 2015 / 005271

[0012] Patent Document 4: Japanese Patent Application Publication No. 2019-059835

[0013] Patent Document 5: Japanese Patent Application Publication No. 2019-089998 Summary of the invention

[0014] Problems to be solved by the invention

[0015] However, when a soluble polyimide is used as in Patent Document 4, the solvent resistance of the obtained molded body is impaired, and it is difficult to fully exhibit the function as a polyimide. Similarly, when a fluorine functional group is introduced as in Patent Document 5, the solubility of the polyimide powder in the solvent is improved, and as a result, the solvent resistance of the obtained molded body is impaired. Therefore, the conventionally known methods cannot fully exhibit the characteristics of the aromatic polyimide powder, and there is a tendency that the solvent resistance and mechanical properties are impaired.

[0016] The present invention aims to solve the above-mentioned problems. In order to prevent the solvent resistance from deteriorating and improve the mechanical properties, repeated experiments were conducted. As a result, surprisingly, it was found that there was a correlation between the amount of volatile components in the aromatic polyimide powder and the mechanical properties of the aromatic polyimide molded body. Therefore, the object of the present invention is to provide an aromatic polyimide powder that can unreservedly and maximally show the characteristics of the aromatic polyimide powder. In particular, the object of the present invention is to provide an aromatic polyimide powder that can be molded into an aromatic polyimide molded body with excellent mechanical properties. In addition, the object of the present invention is to provide a method for improving the mechanical properties of an aromatic polyimide molded body for obtaining a molded body with excellent mechanical properties.

[0017] Means for solving problems

[0018] The present invention particularly relates to the following items.

[0019] 1. An aromatic polyimide powder for a molded body, wherein the content of volatile components contained in the aromatic polyimide powder for a molded body is 0.50 mass % to 5.00 mass % relative to 100 mass % of the aromatic polyimide powder at 25° C. The aromatic polyimide powder for a molded body of the present invention is preferably such that the flexural strength of an aromatic polyimide molded body obtained by molding the aromatic polyimide powder for a molded body of the present invention is 60 MPa or more.

[0020] 2. The method for producing an aromatic polyimide powder for a molded body as described in 1, comprising a volatile component adjustment step as described below: adjusting the ratio of the total amount of volatile components of the aromatic polyimide powder to within a range of 0.50 mass % to 5.00 mass % relative to 100 mass % of the aromatic polyimide powder at 25°C.

[0021] 3. The method for producing an aromatic polyimide powder for a molded body according to 2, wherein the volatile component adjustment step includes a washing step and / or a drying step.

[0022] 4. The method for producing an aromatic polyimide powder for a molded body according to 3, wherein the washing step includes a washing step using alcohol.

[0023] 5. An aromatic polyimide molded product, which is obtained by molding the molded product described in 1 using aromatic polyimide powder, and has a flexural strength of 60 MPa or more.

[0024] 6. A method for improving the mechanical strength of an aromatic polyimide molded product, wherein the content of volatile components contained in an aromatic polyimide powder as a raw material is adjusted to 0.50% by mass to 5.00% by mass based on 100% by mass of the aromatic polyimide powder at 25°C.

[0025] Effects of the Invention

[0026] The present invention can provide an aromatic polyimide powder and a method for producing the same, which can realize an aromatic polyimide molded body having excellent mechanical properties without deteriorating solvent resistance. In addition, a method for improving the mechanical properties of an aromatic polyimide molded body can be provided. According to the present invention, an aromatic polyimide powder that can greatly improve the mechanical strength of a molded body can be obtained by a simple method of adjusting the content of volatile components, which can be said to be an epoch-making invention in industry. DETAILED DESCRIPTION

[0027] <Aromatic polyimide powder for molded articles>

[0028] First, the aromatic polyimide powder for molding of the present invention is described. The aromatic polyimide powder for molding of the present invention contains 0.50 mass% to 5.00 mass% of volatile components. Here, "volatile components" refer to components that volatilize in the temperature range of 50°C to 350°C. In addition, in the present invention, it is characterized in that the volatile components contain 0.50 mass% to 5.00 mass% relative to 100 mass% of the aromatic polyimide powder at 25°C. That is, for example, when the amount of components that volatilize in the temperature range of 50°C to 350°C is 1.00 mass%, the aromatic polyimide powder for molding is composed of 99.00 mass% of components that are non-volatile in the temperature range of 50°C to 350°C, which are mainly composed of aromatic polyimide powder, and 1.00 mass% of components that volatilize in the temperature range of 50°C to 350°C.

[0029] The content of "volatile components" can be determined by thermogravimetric analysis, which is a well-known analytical method. For example, in the case of thermogravimetric analysis, a specified amount of aromatic polyimide powder is heated to a temperature exceeding 350°C at a heating rate of 20°C / min, and the total amount of volatile components volatilized at 50°C to 350°C is measured, and the proportion of the total amount relative to the specified amount of aromatic polyimide powder is calculated. The weight of the aromatic polyimide powder refers to the weight when measured at 25°C. It should be noted that other analytical methods can also be applied as long as the amount of components volatilized in the temperature range of 50°C to 350°C can be measured.

[0030] Such volatile components may be, for example, monomer components such as aromatic diamine components or aromatic tetracarboxylic acid components, residual solvents, additives, water, and modified and decomposed products thereof formed by heating, and the type thereof is not limited. That is, in the present invention, the type of volatile components is meaningless, but the amount of volatile components has technical significance.

[0031] Regarding the content of the component volatilized in the temperature range of 50°C to 350°C of the aromatic polyimide powder for a molded article of the present invention, the lower limit is preferably 1.00% by mass or more, more preferably 1.50% by mass or more, and particularly preferably 2.00% by mass or more, from the perspective of the mechanical properties of the molded article and the handleability of the powder. Similarly, the upper limit is preferably 4.30% by mass or less, more preferably 4.00% by mass or less, and particularly preferably 3.00% by mass or less.

[0032] The aromatic polyimide powder for a molded body of the present invention only needs to have a content of a component volatilizing in a temperature range of 50°C to 350°C within the above range. However, from the perspective of being able to further improve the mechanical properties of the molded body and the handleability of the powder, when the content of a component volatilizing in a temperature range of 50°C to 350°C is set to 100% by mass, the content of a component volatilizing in a temperature range of 150°C to 350°C is preferably 75.0% to 99.0% by mass, and the lower limit is more preferably 80.0% by mass or more, particularly preferably 90.0% by mass or more, and the upper limit is more preferably 98.0% by mass or less, particularly preferably 97.0% by mass or less. In addition, similarly, from the perspective of being able to further improve the mechanical properties of the molded body and the handleability of the powder, when the content of the component volatilizing in the temperature range of 50°C to 350°C is set to 100 mass%, the content of the component volatilizing in the temperature range of 150°C to 250°C is preferably 50.0 mass% to 80.0 mass%, and the lower limit is more preferably 55.0 mass% or more, particularly preferably 60.0 mass% or more, and the upper limit is more preferably 75.0 mass% or less, particularly preferably 70.0 mass% or less.

[0033] The size of the aromatic polyimide powder for the molded body of the present invention is not particularly limited. From the perspective of the mechanical properties of the molded body and the handling properties of the powder, the average particle size is preferably 5 μm to 20 μm. Here, the average particle size referred to in the present invention refers to the value measured using a laser diffraction / scattering particle size distribution measuring device. In addition, as long as the effect of the present invention is achieved, the shape of the aromatic polyimide powder for the molded body is not particularly limited.

[0034] The aromatic polyimide powder for a molded article of the present invention preferably contains an aromatic polyimide containing a repeating unit represented by the following chemical formula (II) as a main component. The method for producing the aromatic polyimide powder will be described later.

[0035] [Chemistry 1]

[0036]

[0037] (In the formula, X1 is one or more tetravalent groups obtained by removing carboxyl groups from tetracarboxylic acids having an aromatic ring, and Y1 is one or more divalent groups obtained by removing amino groups from diamines having an aromatic ring.)

[0038] Among the above X1, a tetravalent group having no substituent on the aromatic ring is preferred, and a tetravalent group represented by chemical formulas (III) to (VII) is particularly preferred.

[0039] [Chemistry 2]

[0040]

[0041] (Wherein, Z1 is a direct bond or the following divalent group:

[0042] [Chemistry 3]

[0043]

[0044] Wherein, W1 in the formula is a divalent organic group, W2 and W3 are each independently an amide bond, an ester bond or a carbonyl bond, and W4 is an organic group containing an aromatic ring.

[0045] Specific examples of W1 include an aliphatic hydrocarbon group having 2 to 24 carbon atoms and an aromatic hydrocarbon group having 6 to 24 carbon atoms.

[0046] Specific examples of W4 include aromatic hydrocarbon groups having 6 to 24 carbon atoms.

[0047] As the compound used as a raw material for forming the tetravalent group represented by the chemical formula (III) to (VII) (also referred to as "aromatic tetracarboxylic acid component" as the case may be), for example, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, diphenylsulfonetetracarboxylic dianhydride, p-terphenyltetracarboxylic dianhydride, m-terphenyltetracarboxylic dianhydride and the like are preferred. The tetravalent group of the acid dianhydride is more preferably derived from 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, benzophenonetetracarboxylic dianhydride, diphenylsulfonetetracarboxylic dianhydride, p-terphenyltetracarboxylic dianhydride, or m-terphenyltetracarboxylic dianhydride, and particularly preferably derived from 3,3',4,4'-biphenyltetracarboxylic dianhydride or 2,3,3',4'-biphenyltetracarboxylic dianhydride, from the perspective of solvent resistance and mechanical properties of the aromatic polyimide molded product. One or more of these aromatic tetracarboxylic acid components can be used.

[0048] Furthermore, a tetracarboxylic acid component having a substituent on the aromatic ring may be used in combination within a range not inhibiting the effects of the present invention. For example, halogen-substituted tetracarboxylic dianhydrides such as 5,5'-[2,2,2-trifluoro-1-[3-(trifluoromethyl)phenyl]ethylene]diphthalic anhydride, 5,5'-[2,2,3,3,3-pentafluoro-1-(trifluoromethyl)propylene]diphthalic anhydride, 1H-difluoro[3,4-b:3',4'-i]xanthene-1,3,7,9(11H)-polyester (Tetoron), 5,5'-oxybis[4,6,7-trifluoro-pyromellitic anhydride], 3,6-bis(trifluoromethyl)pyromellitic dianhydride, 4-(trifluoromethyl)pyromellitic dianhydride, 1,4-difluoropyromellitic dianhydride, and 1,4-bis(3,4-dicarboxytrifluorophenoxy)tetrafluorophthalic anhydride can be mentioned. These tetracarboxylic acid components may be used alone or in combination of two or more, and may be appropriately selected in consideration of the desired properties. The tetracarboxylic acid component having a substituent on the aromatic ring preferably accounts for less than 5 mol% of all tetracarboxylic acid components.

[0049] In addition, among the above Y1, a divalent group having no substituent on the aromatic ring is preferred, and a divalent group represented by chemical formulas (IX) to (X) is particularly preferred.

[0050] [Chemistry 4]

[0051]

[0052] (Wherein, Z2 is a direct bond or the following divalent group:

[0053] [Chemistry 5]

[0054]

[0055] Wherein, W5 to W in formula (XII) 13 Each independently represents a direct bond or any one of the divalent groups represented by the above formula (XI).

[0056] The compound used as the raw material for forming the chemical formula (IX) to (X) (also referred to as "aromatic diamine component" depending on the situation) is preferably p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, etc. From the perspective of solvent resistance of the aromatic polyimide molded product, p-phenylenediamine or 4,4'-diaminodiphenyl ether is more preferably used, and from the perspective of solvent resistance and mechanical properties of the aromatic polyimide molded product, p-phenylenediamine is further preferably used. These aromatic diamine components can be used alone or in combination.

[0057] In addition, within the range that does not hinder the effect of the present invention, a diamine component having a substituent on the aromatic ring can be used in combination. For example, 2,4-toluenediamine, 3,3'-dihydroxy-4,4'-diaminobiphenyl, bis(4-amino-3-carboxyphenyl)methane, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,3,5,6-tetrafluoro-1,4-diaminobenzene, 2,4,5,6-tetrafluoro-1,3-diaminobenzene, 2,3,5,6-tetrafluoro-1,4-benzene(dimethylamine), 2,2'-difluoro(1,1'-biphenyl)-4,4'-diamine, 4,4'-diaminooctafluorobiphenyl, 4,4'-oxybis(2,3,5,6-tetrafluoroaniline) and other halogen-substituted diamines can be used. These diamine components can be used alone or in combination of two or more, and can be appropriately selected in consideration of the desired characteristics. The content of the diamine component having a substituent on the aromatic ring is preferably less than 5 mol% in all diamine components.

[0058] <Method for producing aromatic polyimide powder for molded body>

[0059] Next, a representative example is shown to illustrate the method for producing the aromatic polyimide powder for a molded body of the present invention. The method for producing the aromatic polyimide powder for a molded body of the present invention is not particularly limited as long as the volatile components contained can be adjusted to 0.50 mass % to 5.00 mass %. From the perspective of easy adjustment of the volatile components, an aromatic tetracarboxylic acid component and an aromatic diamine component can be used as raw materials (hereinafter also collectively referred to as "monomer components"), and after forming an aromatic polyimide via a polyamic acid, the volatile components are adjusted, and finally powderized to produce an aromatic polyimide powder for a molded body.

[0060] First, the step of forming the polyamic acid will be described. The polyamic acid particularly preferably includes a repeating unit represented by the following chemical formula (I).

[0061] [Chemistry 6]

[0062]

[0063] (In the formula, A is one or more selected from tetravalent groups obtained by removing a carboxyl group from an aromatic tetracarboxylic acid, and B is one or more selected from divalent groups obtained by removing an amino group from an aromatic diamine.)

[0064] Among the above A, a tetravalent group having no substituent on the aromatic ring is preferred, and a tetravalent group represented by the above chemical formulas (III) to (VII) is particularly preferred.

[0065] As the compound used as a raw material for forming the tetravalent group represented by the chemical formula (III) to (VII) (also referred to as "aromatic tetracarboxylic acid component" as the case may be), for example, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, diphenylsulfonetetracarboxylic dianhydride, p-terphenyltetracarboxylic dianhydride, m-terphenyltetracarboxylic dianhydride and the like are preferred. The tetravalent group of the acid dianhydride is more preferably derived from 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, benzophenonetetracarboxylic dianhydride, diphenylsulfonetetracarboxylic dianhydride, p-terphenyltetracarboxylic dianhydride, or m-terphenyltetracarboxylic dianhydride, and particularly preferably derived from 3,3',4,4'-biphenyltetracarboxylic dianhydride or 2,3,3',4'-biphenyltetracarboxylic dianhydride, from the perspective of solvent resistance and mechanical properties of the aromatic polyimide molded product. One or more of these aromatic tetracarboxylic acid components can be used.

[0066] Furthermore, a tetracarboxylic acid component having a substituent on the aromatic ring may be used in combination within a range not inhibiting the effects of the present invention. For example, halogen-substituted tetracarboxylic dianhydrides such as 5,5'-[2,2,2-trifluoro-1-[3-(trifluoromethyl)phenyl]ethylene]diphthalic anhydride, 5,5'-[2,2,3,3,3-pentafluoro-1-(trifluoromethyl)propylene]diphthalic anhydride, 1H-difluoro[3,4-b:3',4'-i]xanthene-1,3,7,9(11H)-polyester (Tetoron), 5,5'-oxybis[4,6,7-trifluoro-pyromellitic anhydride], 3,6-bis(trifluoromethyl)pyromellitic dianhydride, 4-(trifluoromethyl)pyromellitic dianhydride, 1,4-difluoropyromellitic dianhydride, and 1,4-bis(3,4-dicarboxytrifluorophenoxy)tetrafluorophthalic anhydride can be mentioned. These tetracarboxylic acid components may be used alone or in combination of two or more, and may be appropriately selected in consideration of the desired properties. The tetracarboxylic acid component having a substituent on the aromatic ring preferably accounts for less than 5 mol% of all tetracarboxylic acid components.

[0067] In addition, among the above B, a divalent group having no substituent on the aromatic ring is preferred, and a divalent group represented by the above chemical formulas (IX) to (X) is particularly preferred.

[0068] The compound used as the raw material for forming the chemical formula (IX) to (X) (also referred to as "aromatic diamine component" depending on the situation) is preferably p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, etc. From the perspective of solvent resistance of the aromatic polyimide molded product, p-phenylenediamine or 4,4'-diaminodiphenyl ether is more preferably used, and from the perspective of solvent resistance and mechanical properties of the aromatic polyimide molded product, p-phenylenediamine is further preferably used. These aromatic diamine components can be used alone or in combination.

[0069] In addition, within the range that does not hinder the effect of the present invention, a diamine component having a substituent on the aromatic ring can be used in combination. For example, 2,4-toluenediamine, 3,3'-dihydroxy-4,4'-diaminobiphenyl, bis(4-amino-3-carboxyphenyl)methane, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,3,5,6-tetrafluoro-1,4-diaminobenzene, 2,4,5,6-tetrafluoro-1,3-diaminobenzene, 2,3,5,6-tetrafluoro-1,4-benzene(dimethylamine), 2,2'-difluoro(1,1'-biphenyl)-4,4'-diamine, 4,4'-diaminooctafluorobiphenyl, 4,4'-oxybis(2,3,5,6-tetrafluoroaniline) and other halogen-substituted diamines can be used. These diamine components can be used alone or in combination of two or more, and can be appropriately selected in consideration of the desired characteristics. The content of the diamine component having a substituent on the aromatic ring is preferably less than 5 mol% in all diamine components.

[0070] This polyamic acid uses roughly equimolar aromatic tetracarboxylic acid components and aromatic diamine components, and reacts in a solvent under heating as needed to a desired viscosity (or molecular weight). It should be noted that in the present invention, roughly equimolar means that the molar ratio of the aromatic tetracarboxylic acid component to the aromatic diamine component is about 0.90 to 1.10, preferably about 0.95 to 1.05. In addition, the monomer components used to form the polyamic acid use the above-mentioned aromatic tetracarboxylic acid component and aromatic diamine component as the main components.

[0071] The solvent that can be used in this manufacturing method is not particularly limited, and the known solvent used in the manufacture of polyamic acid can be selected. For example, from the aspect of the solubility of the monomer component or the polyamic acid, it is preferred to include at least one nitrogen-containing solvent. In addition, from the aspect of easy control of the amount of volatile components, a solvent with a boiling point of more than 100°C is preferred. As such a solvent, for example, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, 1,1,3,3-tetramethylurea, 1,3-dimethyl-2-imidazolidinone, N,N-dimethylisobutylamide, N,N-dimethylpropionamide, etc. can be cited.

[0072] Polyamic acid can be formed by adding monomer components and solvent into a reaction vessel equipped with a stirring device and then stirring. There is no particular restriction on the order of adding these raw materials. For example, a predetermined amount of aromatic diamine component can be dissolved in the above-mentioned solvent, and then the aromatic tetracarboxylic acid component can be added; the aromatic tetracarboxylic acid component can also be dissolved in the above-mentioned solvent, and then the aromatic diamine component can be added; the aromatic tetracarboxylic acid component and the aromatic diamine component can also be added alternately. In addition, known additives such as reaction catalysts can be added at any time as needed.

[0073] The reaction temperature is not particularly limited, but is preferably 0 to 100° C., more preferably 10 to 90° C., and still more preferably 20 to 70° C. By adjusting the reaction temperature within the above range, an aromatic polyimide powder with less deviation in coloration and mechanical properties can be produced. The temperature may be constant, or may be appropriately raised or lowered.

[0074] <Formation of Aromatic Polyimide>

[0075] Aromatic polyimide can be formed by a known reaction such as thermal imidization reaction by heating a polyamic acid solution, chemical imidization reaction using an imidizing agent, etc. These imidization reactions are preferably carried out in an inert gas atmosphere by flowing an inert gas such as nitrogen or argon.

[0076] The thermal imidization reaction may be carried out at a reaction temperature appropriately depending on the types of monomer components and the solvent used, and is usually preferably carried out at a temperature in the range of 130°C to 230°C, and more preferably at a temperature in the range of 140°C to 190°C.

[0077] As the imidizing agent for chemical imidization, carboxylic anhydrides such as acetic anhydride, propionic anhydride, succinic anhydride, phthalic anhydride, and benzoic anhydride can be used. From the perspective of cost and easy removal after the reaction, acetic anhydride is preferably used. In addition, the catalyst added when the polyamic acid is formed can be directly utilized, or it can be newly added or additionally added after the polyamic acid is formed. The equivalent of the imidizing agent used is more than the equivalent of the amide bond of the polyamic acid for chemical imidization, preferably 1.1 to 5 times, more preferably 1.5 to 4 times the equivalent of the amide bond. By using an imidizing agent slightly excessive relative to the amide bond in this way, the imidization reaction can be efficiently carried out even at a relatively low temperature.

[0078] From the viewpoint of reducing the variation in the physical properties of the molded product, the imidization rate of the aromatic polyimide (powder) is 95% or more, preferably 98% or more. Here, the imidization rate may be measured by infrared spectroscopy according to a conventional method.

[0079] <Formation of Aromatic Polyimide Powder>

[0080] Finally, the process of manufacturing the aromatic polyimide powder is described. When the aromatic polyimide is formed from the polyamic acid solution as described above, the aromatic polyimide is precipitated as an insoluble substance in the solution system. The powder precipitated in the system is filtered out from the solution, and then subjected to a volatile component adjustment step, thereby obtaining the aromatic polyimide powder.

[0081] The volatile component adjustment process is not particularly limited as long as it can adjust the volatile components of the aromatic polyimide powder, and preferably includes a cleaning process and / or a drying process. In order to improve the efficiency of the cleaning process and / or the drying process, it is preferred to pre-form an aromatic polyimide powder with a particle size close to the desired particle size. For example, the imidization reaction can be carried out under stirring, or a pulverization treatment can be applied after the aromatic polyimide is formed. Of course, two or more of them can also be combined.

[0082] The washing process of the aromatic polyimide powder is not particularly limited to its method, and a known method can be appropriately selected for the washing process. From the perspective of ease of operation, the following washing methods can be appropriately selected: a method of filtering out the aromatic polyimide powder and then rinsing the aromatic polyimide powder remaining in the filter with a washing liquid; a method of placing the aromatic polyimide powder obtained by filtration into a separately prepared container, adding a washing liquid thereto, and stirring the container to wash the aromatic polyimide powder.

[0083] The cleaning liquid used in the cleaning step is not particularly limited as long as it does not dissolve the aromatic polyimide powder, but a hydrophilic solvent such as water or alcohol is preferred.

[0084] There are no particular restrictions on the alcohol used as the cleaning liquid. From the perspective of removing the solvent, imidizing agent, etc. contained in the aromatic polyimide powder, alcohols with a total carbon number of 5 or less, such as methanol, ethanol, and isopropanol, are preferred, and isopropanol is particularly preferred. In addition, from the perspective of controlling volatile components, the cleaning liquid used can be selected to have a boiling point of 150° C. or less, more preferably 100° C. or less. These cleaning liquids can be used alone or mixed with other cleaning liquids as needed.

[0085] The amount of the cleaning liquid relative to the aromatic polyimide powder is not particularly limited, but is preferably 10 times or less of the mass of the aromatic polyimide powder just after filtration from the perspective of industrial productivity. The amount of the cleaning liquid relative to the aromatic polyimide powder referred to here refers to the amount of the cleaning liquid used in one cleaning.

[0086] The drying process of the aromatic polyimide powder can be performed at any temperature, and for example, from the perspective of suppressing the decomposition of the aromatic polyimide powder, it is preferably 400° C. or less, more preferably 350° C. or less, further preferably 300° C. or less, and particularly preferably 200° C. or less. The lower limit temperature can be preferably set to 80° C. or more, more preferably 100° C. or more, and particularly preferably 110° C. or more.

[0087] In addition, the drying of the aromatic polyimide powder can be carried out under normal pressure or under reduced pressure. In addition, it can be carried out under the atmosphere or under an inert gas atmosphere. From the aspect of suppressing the decomposition of the aromatic polyimide powder, it is preferably carried out under an inert gas atmosphere. In addition, it can be carried out under a mixed atmosphere of the atmosphere and the inert gas, or it can be carried out under the atmosphere and then under the inert gas atmosphere, or it can be carried out under the inert gas atmosphere and then under the atmosphere.

[0088] The drying time can be appropriately adjusted in consideration of the content of the volatile components. Among them, from the perspective of suppressing the decomposition of the aromatic polyimide powder and industrial productivity, it is preferably carried out within 36 hours, more preferably within 24 hours, and particularly preferably within 18 hours. The lower limit of the drying time is not particularly limited, but is preferably 30 minutes or more, and more preferably 1 hour or more.

[0089] Such a cleaning process and / or drying process may be repeated multiple times, and the cleaning process and the drying process may be repeated alternately. In the case of including multiple cleaning processes or drying processes, the multiple cleaning processes or drying processes do not need to be performed under the same conditions, and the conditions may be appropriately changed. For example, the type of cleaning liquid and the amount of the cleaning liquid relative to the aromatic polyimide powder may be changed in the cleaning process, and the drying temperature, drying time, etc. may also be changed in the drying process.

[0090] In the usual cleaning process and / or drying process, not limited to polyimide powder, other resin powders, etc. are also committed to excluding volatile components as much as possible. However, in the present invention, the volatile component adjustment process including the cleaning process and / or drying process is different in that the content of the volatile component is adjusted to 0.5% by mass to 5.0% by mass. Therefore, in order to distinguish it from the usual cleaning process and / or drying process, it is called the volatile component adjustment process in the present invention. For example, in the case of industrial production of aromatic polyimide powder, the scale of the manufacturing equipment is large and the amount of raw materials used is large, so it is predicted that the aromatic polyimide powder with a volatile component content of less than 0.5% by mass can be obtained in whole or in part. For such an aromatic polyimide powder with a volatile component content of less than 0.5% by mass, the above-mentioned organic solvent, etc., which is sprayed in the desired amount, can be made 0.5% by mass to 5.0% by mass. That is, the volatile component adjustment process is a concept that includes not only a process for reducing the content of volatile components, but also a process for increasing the content of the above-mentioned volatile components. It is reiterated that the volatile component adjustment step is a step of making the content of the volatile component 0.5 mass % to 5.0 mass %. It should be noted that, as the organic solvent for spraying, in addition to the above-mentioned organic solvents, various organic solvents such as acetone, methyl ethyl ketone, toluene, methanol, ethanol, isopropanol, ethyl benzoate, ethylene glycol, and propylene glycol can also be used. In addition, after the spraying of the organic solvent, it can be dried as needed. In addition, the following method can also be used: the aromatic polyimide powder is mixed with the above-mentioned organic solvent and dried to adjust the content of the volatile component.

[0091] <Aromatic polyimide molded article and method for producing the same>

[0092] The aromatic polyimide molded body of the present invention is formed by molding the above-mentioned molded body of the present invention with aromatic polyimide powder, and has a mechanical property of a bending strength of 60 MPa or more. Here, the bending strength referred to in the present invention is obtained by measuring the breaking strength of the molded body molded under the following conditions using a bending strength tester with n=10 times and calculating the average value. After the powder is filled into the powder molding machine, the powder is subjected to a 6000 kgf / cm 2The pressure of uniaxial molding is used to form a rectangular parallelepiped shape of 5mm in width × 40mm in length × 4mm in thickness. The object formed into the rectangular parallelepiped is fired at a temperature of 400°C in an air atmosphere without pressure, thereby producing a molded body. For the molded body thus produced, a bending strength tester is used to measure the test speed of 0.5mm / min, and the strength at break is taken as the breaking strength. The bending strength is preferably 62MPa or more, more preferably 64MPa or more, and further preferably 65MPa or more. It should be noted that at this time, as the condition for non-pressure firing, it is set to 400°C in an air atmosphere, and other conditions are not particularly limited. Representatively, the following conditions can be set: heating at 10°C / min, keeping at a temperature of 50°C for 30 minutes, heating again at 10°C / min, keeping at a temperature of 200°C for 1 hour, then heating at 10°C / min, and keeping at a temperature of 400°C for 15 minutes. In addition, the molding time in uniaxial molding can be representatively set to 1 minute.

[0093] In order to have such bending strength, as long as the aromatic polyimide powder of the present invention is used, its manufacturing method is not particularly limited, and the aromatic polyimide powder of the present invention is supplied to the manufacturing of the molded body in a state where the amount of volatile components is within the above range. For example, the aromatic polyimide powder of the present invention can be filled into a mold, and pressure and heat can be applied simultaneously or separately to perform heating and compression, thereby manufacturing. That is, the aromatic polyimide molded body of the present invention can be an aromatic polyimide sintered molded body molded and sintered by heating and compression. Such heating temperature and pressure conditions depend on the molding device, and the range suitable for the device can be arbitrarily selected. In particular, in the manufacturing method of the present invention, since the volatile components are contained in a specific range, the heat resistance of the aromatic polyimide can be fully exerted. As a result, molding can be performed at a temperature above 300°C, and even if molding is performed at a high temperature of 400°C or above, the appearance of the molded body will not deteriorate and cracks will not occur, and the desired mechanical strength can be exhibited. The upper limit of the heating temperature is preferably below 600°C, more preferably below 550°C, and particularly preferably below 500°C.

[0094] Similarly, the pressure can be selected in the optimal range suitable for the manufacturing device. From the perspective of improving the mechanical properties of the aromatic polyimide molded body and suppressing the occurrence of cracks in the aromatic polyimide molded body, 4000 kgf / cm 2 More preferably, 5000 kgf / cm 2 More than 5500kgf / cm 2 Above, preferably 7000kgf / cm 2 Less than, more preferably 6500kgf / cm 2The heating compression molding time in the heating compression molding is preferably 10 minutes or more, more preferably 40 minutes or more, preferably 100 minutes or less, more preferably 60 minutes or less. Furthermore, from the perspective of improving the mechanical properties of the aromatic polyimide molded body and suppressing the generation of cracks in the aromatic polyimide molded body, the molded body subjected to heating compression molding is preferably cooled in the mold at a rate of 5°C / min to 10°C / min. On the other hand, the compression molding time in the compression molding at room temperature is preferably 30 seconds or more, more preferably 1 minute or more, preferably 10 minutes or less, more preferably 5 minutes or less.

[0095] In addition, the aromatic polyimide molded body of the present invention can also be manufactured by compression molding at the above-mentioned pressure at room temperature and then sintering under non-compression. That is, the aromatic polyimide molded body of the present invention can be an aromatic polyimide sintered molded body that is sintered after molding. At this time, from the perspective of the mechanical properties of the aromatic polyimide molded body, the sintering temperature is preferably 300°C or more, more preferably 350°C or more, particularly preferably 400°C or more, preferably 600°C or less, more preferably 550°C or less, and particularly preferably 500°C or less. The sintering time when sintering is performed under non-compression is preferably 60 minutes or more, more preferably 120 minutes or more, preferably 240 minutes or less, and more preferably 180 minutes or less. From the perspective of improving the mechanical properties of the aromatic polyimide molded body and suppressing the generation of cracks in the molded body, the sintered molded body is preferably cooled at a rate of 5°C / min to 10°C / min.

[0096] It should be noted that when sintering is performed under non-compression, the sintering temperature can be set to the above temperature, and the heating rate during sintering is preferably 5°C / minute or more, more preferably 10°C / minute or more, preferably 30°C / minute or less, and more preferably 20°C / minute or less. In addition, when sintering is performed under non-compression, a temperature holding treatment for maintaining the temperature can be performed during the heating process. As a temperature holding treatment, during the heating process, it can be performed once or multiple times. For example, in the case of performing three temperature holding treatments, the holding temperature in the second temperature holding treatment is preferably 100°C or more, more preferably 150°C or more, preferably 250°C or less, and more preferably 200°C or less, and the holding time is preferably 10 minutes or more, more preferably 30 minutes or more, preferably 120 minutes or less, and more preferably 60 minutes or less. In addition, the holding temperature in the third temperature holding treatment is preferably above 350°C, more preferably above 400°C, preferably below 550°C, more preferably below 500°C, and the holding time is preferably above 5 minutes, more preferably above 15 minutes, preferably below 60 minutes, more preferably below 30 minutes.

[0097] In addition, when manufacturing the above-mentioned aromatic polyimide molded body, any filler can be mixed with the above-mentioned aromatic polyimide powder for use. The filler material used is not particularly limited, and inorganic fillers such as glass fiber, ceramic fiber, boron fiber, glass beads, whiskers, diamond powder, aluminum oxide, silicon dioxide, natural mica, synthetic mica, aluminum oxide, carbon black, silver powder, copper powder, aluminum powder, nickel powder, metal fiber, ceramic fiber, whiskers, silicon carbide, silicon oxide, aluminum oxide, magnesium powder, titanium powder, carbon fiber, graphite, or organic fillers such as fluorine-containing resin and aramid fiber can be used. These fillers can be used alone or in the form of a combination of two or more fillers.

[0098] The amount of the filler used can be selected according to the application, and for example, it can be used in the range of 1% by mass to 50% by mass based on the weight of the aromatic polyimide powder.

[0099] In the above-mentioned heating and compression molding, as an apparatus for manufacturing the aromatic polyimide molded body, for example, a four-column hydraulic press, a high-pressure hot press, a WIP device, etc. can be cited. In addition, the above-mentioned preform is preferably formed by a method using, for example, Wet-CIP, Dry-CIP, a high-pressure press, a hydraulic press, a rotary press, and a tablet press. In addition, the aromatic polyimide molded body of the present invention can also be manufactured by applying the above-mentioned heating and compression molding method to a sheet-like laminate.

[0100] Thus, the aromatic polyimide powder of the present invention can fully exert the characteristics of aromatic polyimide, and thus can be applied to a variety of production methods, and the conditions thereof are also wide, and from this point of view, the industrial utilization value is high. In particular, the aromatic polyimide powder can also exert excellent mechanical properties by a method in which the aromatic polyimide powder is compression-molded at room temperature at the above-mentioned pressure and then sintered under non-compression (so-called direct forming), and therefore, according to the present invention, aromatic polyimide molded bodies having various shapes can be manufactured with high productivity.

[0101] The aromatic polyimide molded product obtained by the present invention can be suitably used as pins, guides, evaluation sockets, vacuum pads, etc. of semiconductor manufacturing-related equipment, bushings, seals, thrust washers, bearing supports, piston rings, lock nut inserts, etc. for automobile / aerospace purposes, and bearing sleeves, roller bushings, piston rings, etc. for industrial machinery-related equipment.

[0102] Example

[0103] Hereinafter, the present invention will be described in more detail with reference to Examples, Comparative Examples and Reference Examples, but the present invention is not limited to these Examples.

[0104] The measurement method used in the following examples is shown.

[0105] <Volatile content>

[0106] About 20 mg of aromatic polyimide powder was used as a test sample, and the temperature was raised from 25°C to 700°C at a heating rate of 20°C / min in a nitrogen atmosphere using a thermogravimetric measuring apparatus. The weight reduction rate at 50°C to 350°C was calculated from the obtained weight curve. In addition, the weight reduction rate at 150°C to 250°C and the weight reduction rate at 150°C to 350°C were also calculated.

[0107] <Average particle size>

[0108] About 20 mg of the aromatic polyimide powder was used as a test sample, and the average particle size was measured using a laser diffraction / scattering particle size distribution analyzer.

[0109] <Bending Strength>

[0110] For aromatic polyimide powder, a powder molding machine was used at room temperature at 6000 kgf / cm 2 The obtained aromatic polyimide molded body was subjected to uniaxial molding for 1 minute under a pressure of 1000 g / cm, thereby obtaining a 5 mm wide × 40 mm long × 4 mm thick aromatic polyimide molded body. After that, the obtained aromatic polyimide molded body was subjected to non-pressure sintering under the prescribed temperature conditions described later in an air atmosphere, and then measured using a bending strength tester at a test speed of 0.5 mm / min. The measurement was performed n=10 times, and the average value was taken as the bending strength.

[0111] The abbreviations of the compounds used in the following examples are as follows.

[0112] s-BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0113] a-BPDA: 2,3,3',4'-biphenyltetracarboxylic dianhydride

[0114] PMDA: 1,2,4,5-benzenetetracarboxylic dianhydride

[0115] ODPA: 4,4'-oxydiphthalic anhydride

[0116] PPD: p-phenylenediamine

[0117] NMP: N-methyl-2-pyrrolidone

[0118] IPA: Isopropyl alcohol

[0119] <Preparation of Aromatic Polyimide Powder A>

[0120] Add 240.00g of NMP as a solvent, add 28.56g of s-BPDA, 2.15g of a-BPDA, and 11.29g of PPD, and stir to dissolve. Then, heat to 50°C for polymerization to obtain a polyamic acid solution. Thereafter, further heat to 190°C for imidization reaction to precipitate aromatic polyimide powder. Filter out the precipitated powder, wash it 4 times with IPA, and dry it at 100°C for 24 hours under a reduced pressure of 2kPa to obtain aromatic polyimide powder A. The volatile component amount of the obtained aromatic polyimide powder A (the content of the component that volatilizes in the temperature range of 50°C to 350°C, the same below) is 1.03% by mass. The content of components volatilizing in the temperature range of 150°C to 350°C was 0.99 mass % (96.1 mass % of the total volatile components), and the content of components volatilizing in the temperature range of 150°C to 250°C was 0.61 mass % (59.2 mass % of the total volatile components).

[0121] <Preparation of Aromatic Polyimide Powder B>

[0122] In the same manner as in the preparation of aromatic polyimide powder A, after the aromatic polyimide powder was precipitated, the precipitated powder was filtered out, washed with IPA four times, and dried at 120° C. for 2 hours in a nitrogen atmosphere to obtain aromatic polyimide powder B. The volatile content of the obtained aromatic polyimide powder B was 1.50% by mass. In addition, the content of the component volatilizing in the temperature range of 150° C. to 350° C. was 1.23% by mass (82.0% by mass in the total volatile content), and the content of the component volatilizing in the temperature range of 150° C. to 250° C. was 0.78% by mass (52.0% by mass in the total volatile content).

[0123] <Preparation of Aromatic Polyimide Powder C>

[0124] In the same manner as in the preparation of the aromatic polyimide powder A, the aromatic polyimide powder was precipitated, the precipitated powder was filtered out, washed with IPA three times, and dried at 120° C. for 2 hours in a nitrogen atmosphere to obtain an aromatic polyimide powder C. The volatile content of the obtained aromatic polyimide powder C was 2.10% by mass. In addition, the content of the component volatilizing in the temperature range of 150° C. to 350° C. was 1.97% by mass (93.8% by mass in the total volatile content), and the content of the component volatilizing in the temperature range of 150° C. to 250° C. was 1.51% by mass (71.9% by mass in the total volatile content).

[0125] <Preparation of Aromatic Polyimide Powder D>

[0126] In the same manner as in the preparation of the aromatic polyimide powder A, the aromatic polyimide powder was precipitated, the precipitated powder was filtered out, washed twice with IPA, and dried at 120° C. for 2 hours in a nitrogen atmosphere to obtain an aromatic polyimide powder D. The volatile content of the obtained aromatic polyimide powder D was 4.23% by mass. In addition, the content of the component volatilizing in the temperature range of 150° C. to 350° C. was 3.27% by mass (77.3% by mass in the total volatile content), and the content of the component volatilizing in the temperature range of 150° C. to 250° C. was 2.81% by mass (66.4% by mass in the total volatile content).

[0127] <Preparation of Aromatic Polyimide Powder E>

[0128] After the aromatic polyimide powder was precipitated in the same manner as in the preparation of the aromatic polyimide powder A, the precipitated powder was filtered out, washed four times with IPA, and dried at 260° C. for 8 hours in a nitrogen atmosphere to obtain an aromatic polyimide powder E. The volatile content of the obtained aromatic polyimide powder E was 0.08% by mass.

[0129] <Preparation of Aromatic Polyimide Powder F>

[0130] In the same manner as in the preparation of aromatic polyimide powder A, the aromatic polyimide powder was precipitated, the precipitated powder was filtered out, washed four times with IPA, and dried at 250° C. for 24 hours under a reduced pressure of 2 kPa to obtain aromatic polyimide powder F. The volatile content of the obtained aromatic polyimide powder F was 0.20% by mass.

[0131] <Preparation of Aromatic Polyimide Powder G>

[0132] In the same manner as in the preparation of aromatic polyimide powder A, the aromatic polyimide powder was precipitated, the precipitated powder was filtered out, washed four times with IPA, and dried at 225° C. for 18 hours under a reduced pressure of 2 kPa to obtain aromatic polyimide powder G. The volatile content of the obtained aromatic polyimide powder G was 0.49% by mass.

[0133] <Preparation of Aromatic Polyimide Powder H>

[0134] In the same manner as in the preparation of aromatic polyimide powder A, the aromatic polyimide powder was precipitated, the precipitated powder was filtered out, washed once with IPA, and then dried at 100° C. for 24 hours under a reduced pressure of 2 kPa to obtain aromatic polyimide powder H. The volatile content of the obtained aromatic polyimide powder H was 5.62% by mass.

[0135] <Preparation of Aromatic Polyimide Powder I>

[0136] In the same manner as in the preparation of aromatic polyimide powder A, the aromatic polyimide powder was precipitated, the precipitated powder was filtered out, washed once with IPA, and then dried at 120° C. for 2 hours in a nitrogen atmosphere to obtain aromatic polyimide powder I. The volatile content of the obtained aromatic polyimide powder I was 10.49% by mass.

[0137] <Preparation of Aromatic Polyimide Powder J>

[0138] After the aromatic polyimide powder was precipitated in the same manner as in the preparation of the aromatic polyimide powder A, the precipitated powder was filtered out and then dried at 120° C. for 2 hours in a nitrogen atmosphere to obtain an aromatic polyimide powder J. The volatile content of the obtained aromatic polyimide powder J was 50.00% by mass.

[0139] <Preparation of Aromatic Polyimide Powder K>

[0140] 7 g of the aromatic polyimide powder A obtained by the above method was prepared, 1 g of ethyl benzoate and 29 g of acetone were added, and stirred. Then, the aromatic polyimide powder to which ethyl benzoate and acetone were added was dried at 120° C. for 2 hours under a nitrogen atmosphere to obtain an aromatic polyimide powder K. The volatile content of the obtained aromatic polyimide powder K was 0.98% by mass.

[0141] <Preparation of Aromatic Polyimide Powder L>

[0142] 6 g of the aromatic polyimide powder A obtained by the above method was prepared, 1 g of NMP and 29 g of acetone were added, and stirred. Then, the aromatic polyimide powder to which NMP and acetone were added was dried at 120° C. for 2 hours under a nitrogen atmosphere to obtain an aromatic polyimide powder L. The volatile content of the obtained aromatic polyimide powder L was 4.13% by mass.

[0143] <Example 1>

[0144] The obtained aromatic polyimide powder A was filled into a mold and heated at room temperature at 6000 kgf / cm using a powder molding machine. 2The obtained aromatic polyimide molded body was subjected to uniaxial molding for 1 minute at a pressure of 50°C to obtain an aromatic polyimide molded body with a width of 5 mm × a length of 40 mm × a thickness of 4 mm. The obtained aromatic polyimide molded body was subjected to non-pressure firing at 400°C in an atmospheric atmosphere, and the bending strength was evaluated. The results obtained are shown in Table 1. It should be noted that the specific conditions for firing are as follows. That is, the temperature is increased at 10°C / min, maintained at a temperature of 50°C for 30 minutes, and then the temperature is increased at 10°C / min again, maintained at a temperature of 200°C for 1 hour, then the temperature is increased at 10°C / min, maintained at a temperature of 400°C for 15 minutes, and then cooled at 10°C / min.

[0145] <Example 2>

[0146] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that the aromatic polyimide powder B was used instead of the aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 1.

[0147] <Example 3>

[0148] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that the aromatic polyimide powder C was used instead of the aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 1.

[0149] <Example 4>

[0150] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that the aromatic polyimide powder D was used instead of the aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 1.

[0151] <Comparative Example 1>

[0152] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that the aromatic polyimide powder E was used instead of the aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 2.

[0153] <Comparative Example 2>

[0154] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that aromatic polyimide powder F was used instead of aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 2.

[0155] <Comparative Example 3>

[0156] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that the aromatic polyimide powder G was used instead of the aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 2.

[0157] <Comparative Example 4>

[0158] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that the aromatic polyimide powder H was used instead of the aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 2.

[0159] <Comparative Example 5>

[0160] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that the aromatic polyimide powder I was used instead of the aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 2.

[0161] <Comparative Example 6>

[0162] The molding was attempted to be carried out in the same procedure as in Example 1 except that the aromatic polyimide powder J was used instead of the aromatic polyimide powder A. However, the molding could not be carried out smoothly (molding was impossible).

[0163] <Example 5>

[0164] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that the aromatic polyimide powder K was used instead of the aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 3.

[0165] <Example 6>

[0166] An aromatic polyimide molded product was obtained in the same manner as in Example 1 except that the aromatic polyimide powder L was used instead of the aromatic polyimide powder A. The bending strength of the obtained aromatic polyimide molded product was evaluated. The obtained results are shown in Table 3.

[0167] <Example 7>

[0168] In the same manner as in Example 1, the aromatic polyimide powder A was used to perform uniaxial molding, thereby obtaining an aromatic polyimide molded body of 5 mm in width × 40 mm in length × 4 mm in thickness. The obtained molded body was then subjected to non-pressure firing under the conditions shown in Table 4 in an air atmosphere, and the bending strength was evaluated. The obtained results are shown in Table 4.

[0169] <Example 8>

[0170] In the same manner as in Example 1, the aromatic polyimide powder A was used to perform uniaxial molding, thereby obtaining an aromatic polyimide molded body of 5 mm in width × 40 mm in length × 4 mm in thickness. The obtained molded body was then subjected to non-pressure firing under the conditions shown in Table 4 in an air atmosphere, and the bending strength was evaluated. The obtained results are shown in Table 4.

[0171] [Table 1]

[0172] Table 1

[0173]

[0174] [Table 2]

[0175] Table 2

[0176]

[0177] [Table 3]

[0178] Table 3

[0179]

[0180] [Table 4]

[0181] Table 4

[0182]

[0183] The solvent resistance of the obtained molded bodies was evaluated. As a result, the molded bodies formed by molding the aromatic polyimide powders of Examples 1 to 8 had excellent solvent resistance comparable to that of the molded bodies formed by molding the aromatic polyimide powders of Comparative Examples 1 to 3 having a small volatile component content. On the other hand, as the volatile component content increased, the solvent resistance deteriorated.

[0184] Industrial Applicability

[0185] The aromatic polyimide powder of the present invention can provide an aromatic polyimide molded product having excellent mechanical properties without deteriorating solvent resistance, and can also provide a method for improving the mechanical strength of an aromatic polyimide molded product.

Claims

1. An aromatic polyimide powder for a molded body, which is an aromatic polyimide powder for a molded body containing an aromatic polyimide containing a unit derived from 2,3,3',4'-biphenyltetracarboxylic dianhydride as a main component, wherein: The aromatic polyimide powder for molding has a volatile component content of 0.50 to 5.00 mass % relative to 100 mass % of the aromatic polyimide powder at 25° C., and the aromatic polyimide molding obtained by molding has a flexural strength of 60 MPa or more.

2. The method for producing an aromatic polyimide powder for a molded body according to claim 1, comprising a volatile component adjustment step as described below: adjusting the ratio of the total amount of volatile components of the aromatic polyimide powder to be within the range of 0.50 mass % to 5.00 mass % relative to 100 mass % of the aromatic polyimide powder at 25°C.

3. The method for producing an aromatic polyimide powder for a molded body according to claim 2, wherein: The volatile component adjustment step includes a washing step and / or a drying step.

4. The method for producing an aromatic polyimide powder for a molded article according to claim 3, wherein: The cleaning step includes a cleaning step using alcohol.

5. An aromatic polyimide molded body, which is obtained by molding the molded body according to claim 1 using an aromatic polyimide powder, and has a flexural strength of 60 MPa or more.

6. A method for improving the mechanical strength of an aromatic polyimide molded product, which is a method for improving the mechanical strength of an aromatic polyimide molded product containing an aromatic polyimide containing units derived from 2,3,3',4'-biphenyltetracarboxylic dianhydride as a main component, wherein: The content of the volatile component contained in the aromatic polyimide powder as a raw material is adjusted to 0.50 mass % to 5.00 mass % based on 100 mass % of the aromatic polyimide powder at 25°C.